Fabrication and Characterization of 3D-Printed Polylactide Composite Scaffolds with Modified Graphene

Worathep Khimlek †,‡, Jirawan Jindakeaw §, Vitsarut Primpray ∥, Chanpen Karuwan ∥, Teruoki Tago ⊥, Paiboon Sreearunothai †, Chariya Kaewsaneha †, Adisorn Tuantranont #, Pakorn Opaprakasit †,*
PMCID: PMC13756721  PMID: 43023010

Abstract

In this study, we introduce novel multifunctional biomaterial inks for extrusion-based 3D bioprinting to create scaffolds for potential tissue engineering. This study focuses on developing composite materials by incorporating alkyl ketene dimer (AKD)-modified graphene nanoplatelets (GP) into polylactide (PLA) using a solvent casting technique. GP was synthesized via electrolytic exfoliation in an aqueous poly­(sodium 4-styrenesulfonate) solution and subsequently modified with AKD by ball milling to enhance dispersion and PLA compatibility. Physical and chemical characterization confirmed the successful synthesis and structural properties of the AKD-modified GP. PLA-GPD20 films containing 20 wt % AKD-modified GP exhibited significantly improved elongation at break and maintained tensile strength comparable to neat PLA. All biomaterial composite films exhibited high stiffness, as evidenced by glass transition temperatures above room temperature, and electrical conductivity in the semiconductor range. The results highlight the significant positive impact of AKD on the physical and electrical properties, as well as the printability, of the composites. The printability performance potential was evaluated using 10 wt % PLA-GPD20 biomaterial inks to generate scaffolds with different patterns. The mechanical testing of the printed scaffolds revealed that the tensile strength and modulus increased with the incorporation of GPD20. The printing orientation is an effective parameter for tuning the balance between stiffness and ductility; scaffolds printed at 90° exhibited higher Young’s modulus but lower elongation at yield and tensile strength than those printed at 45°. Furthermore, incorporating AKD into GP/PLA composites improved hydrophobicity. The results suggest that AKD-modified graphene composites hold substantial promise for the development of advanced multifunctional materials for tissue engineering applications.


graphic file with name ao6c04916_0013.webp


graphic file with name ao6c04916_0011.webp

1. Introduction

Three-dimensional (3D) bioprinting has transformed biomedical and tissue engineering by enabling the precise fabrication of scaffolds with customizable pore sizes and complex internal geometries. One of the major advantages of 3D bioprinting is its ability to produce patient-specific constructs with tailored mechanical properties and interconnected networks that closely mimic natural tissue. − As temporary structures, biomaterial scaffolds play a key role in supporting the growth and regeneration of damaged tissues and organs. These materials are valuable for bone, cartilage, and skin regeneration applications. , However, scaffold substitutes must be considered to maintain their shape and safely degrade into nontoxic byproducts. , Polylactide (PLA) is a degradable aliphatic polyester derived from renewable agricultural resources, such as corn, cassava, and sugar cane. PLA is a promising biocompatible polymer approved by the U.S. Food and Drug Administration as a biomedical material, coupled with excellent solubility and easy processing across various organic solvents. This makes it adaptable to various tissue types. , PLA can be tuned to achieve a prolonged degradation rate, making it suitable for developing biodegradable devices intended for long-term use that are tailored to match specific biodegradation timelines with tissue healing time. , Although PLA offers many advantages, it still faces certain limitations, such as low toughness and limited plastic deformation, which restrict its broader use in load-bearing or mechanically demanding applications. −

Incorporating reinforcement materials is a promising solution to address these challenges and enhance the mechanical properties. − Graphene nanoplatelets (GP) stand out as an outstanding choice for improving the properties of PLA-based biopolymers. GP is a two-dimensional carbon-based material that is one of the strongest and lightest materials. It exhibits exceptional electrical conductivity, high fracture toughness, high thermal stability, and high surface area. , GP and its derivatives have been widely used as additives, particularly in tissue engineering, as these materials promote specific cell behaviors and facilitate noncovalent interactions with biomolecules via oxygenated groups on their surfaces. However, the toxicity of GP remains a crucial consideration from a tissue engineering perspective, as it directly governs its suitability for use in contact with cells and tissues, and is highly dependent on factors such as surface chemistry and concentration. Recent studies have reported the development of GP-reinforced biopolymers, particularly for application as scaffolds in tissue-engineered constructs. Soltani et al. developed a 3D-printed PLA/poly­(ε-caprolactone) (PCL) blend by incorporating 1.5 wt % GP. The 3D-printed composites exhibited significant enhancements in mechanical stiffness and electrical conductivity. These improved properties render the developed material highly suitable for specific biomedical applications, especially in nerve tissue regeneration, where both structural support and electrical signal transduction are critical. Seyedsalehi et al. developed a 3D-printed PCL/reduced graphene oxide (rGO) with controlled geometry and internal architecture. The resulting materials exhibited excellent cytocompatibility and favorable biological properties. However, achieving the optimal GP-based material loading was challenging, as excessive amounts led to extrusion issues caused by GP sheet aggregation. This aggregation is primarily attributed to the intermolecular van der Waals interactions between the GP layers and their limited solubility in certain organic solvents. , A promising approach to this challenge involves incorporating compatibilizers, certain polymers, and surfactants to modify and improve GP dispersion in composite materials. These additives help mitigate aggregation and improve the compatibility, dispersion stability, and interfacial interaction of GP platelets within a polymer matrix. −

Alkyl ketene dimer (AKD), an inexpensive biobased organic compound, is an effective compatibilizer and dispersant across diverse applications. Its primary function is to lower the interfacial energy, which is critical for achieving uniform component dispersion within a polymer matrix and inhibiting aggregation. This attribute enhances the performance of composite materials, even at low incorporation levels, and facilitates effective dispersion in water-insoluble solvents. In addition, the long alkyl chains of AKD impart hydrophobicity to surface materials, and its nontoxic nature, coupled with its use in FDA-approved food-safe materials, expands its utility. However, research into the application of AKD as an interfacial modifier to enhance compatibility in immiscible biopolymer blends remains limited.

Despite significant progress in developing biobased materials and conductive fillers for tissue engineering, achieving a balanced combination of printability, mechanical robustness, electrical functionality, and interfacial compatibility remains a major challenge for extrusion-based 3D bioprinting. In particular, the poor dispersion of graphene-based nanomaterials in polymer matrices and their limited compatibility with biodegradable polymers, such as PLA, often hinder the realization of multifunctional scaffolds with reliable performance. To address these limitations, this study proposes a strategy that incorporates AKD-modified GP into a PLA matrix to develop advanced biomaterial ink systems. The AKD modification is expected to enhance filler dispersion, improve interfacial interactions, and tailor surface properties, thereby enabling improved mechanical and electrical performance and printability. Accordingly, this work aims to (i) synthesize and characterize AKD-modified GP, (ii) investigate the structure–property relationships of PLA-based composites, and (iii) evaluate their printability and mechanical performance in extrusion-based 3D-printed scaffolds. The outcomes of this study are expected to provide new insights into the design of multifunctional biobased composites for potential use in tissue engineering.

2. Experimental Section

2.1. Materials

Polylactide (PLA, 4043D) pellet was supplied by NatureWorks. Graphite rods with a technical grade, dia.1/4″ (6.2 mm) × 12″ (304 mm), were purchased from Electron Microscopy Science USA and were used as raw material to synthesize graphene. Poly­(sodium 4-styrenesulfonate) (PSS, Mw = 70,000) was obtained from Sigma-Aldrich, USA. Chloroform (grade AR, 99.9%) was purchased from Carlo Erba Reagents. Alkyl ketene dimer (AKD) was provided by Kemira, Thailand.

2.2. Graphene Synthesis and Modification

GP was synthesized via an electrolytic exfoliation method as previously reported. , An electrolyte solution was prepared by dissolving 0.1 wt % PSS in DI water. Two graphite (GH) rods were employed as the working electrode (anode) and the counter electrode (cathode) and were placed in the prepared electrolyte solution, as shown in Figure a. A constant voltage of 8 V was applied between the electrodes at room temperature. The anode graphite rod was oxidized during the electrolysis process. The solution darkened, with a black precipitate in the reaction cell, and gas evolution was driven by electrochemical reactions at the electrode surfaces (Figure b). The process was continued until the graphite anode rod was fully consumed. The synthesized GP was collected by vacuum filtration and thoroughly washed with DI water and ethanol to remove residual salts. The obtained product was dried in an oven at 80 °C for 24 h.

1.

1

(a) Experimental setup of graphene electrolytic exfoliation and (b) proposed electrolytic exfoliation mechanisms.

During the modification process, the as-exfoliated GP was mixed and reacted with AKD at different ratios (0, 5, 10, 20, and 30 wt %) using a ball milling machine (Retsch model Emax). Each mixture was processed in 50 mL Zirconium oxide grinding jars with balls (Ø = 5 mm). Milling was performed under a ball-to-powder mass ratio of 40:1 at 1000 rpm for 1 h. The final AKD-modified GP product (GPD) was sieved through a 400-mesh stainless steel screen to separate and collect the desired particle fractions. The samples are referred to as GPDxx according to their corresponding AKD content.

2.3. Preparation of PLA/GPD Composite Films

The PLA/GPD biopolymer composite films were fabricated using a solution casting method. GPD was dispersed in 10 mL of chloroform at various concentrations (0, 5, 10, 15, 20, and 30 wt %) and sonicated for 1 h at 25 °C. Subsequently, 0.8 g of dried PLA pellets were slowly added to the prepared dispersion under ambient conditions to achieve complete dissolution. The homogeneous mixture was degassed and cast on Teflon plates. All composite films were fabricated via air-drying, followed by oven-drying at 50 °C for 48 h to remove residual solvent.

2.4. Biomaterial Ink Preparation and 3D Bioprinting Fabrication

The PLA/GPD composite scaffolds were fabricated using an extrusion-based 3D printer (4th generation 3D Bioplotter, Envisiontec, Germany). GPD20 was selected as a suitable additive for ink preparation due to its optimal modification efficiency. The material was incorporated into a 40% (wt/vol) PLA/chloroform solution at 0 and 10 wt % and thoroughly homogenized. After degassing, the resulting ink was filled into a pneumatic cartridge. The biomaterial ink was extruded with two different raster orientations: 45° (45/–45) and 90° (0/90), in a rectangular block model. The bioprint layout followed a specimen shape with dimensions of 10 × 90 mm2, a dispensing line spacing of 100 μm, and an extrusion pressure ranging from 1.8 to 2.3 bar. The nozzle operated at a speed of 18–20 mm/s, with an inner tip diameter of 0.41 mm. The material was deposited layer by layer for 5 layers. The scaffold samples were dried at room temperature for 24 h after printing to ensure complete solvent evaporation.

2.5. Characterization

The effects of chemical constituents/compositions, number of printed layers, and size of GP/GPD on the structures and properties of the resulting printed products were evaluated using high-resolution Raman spectroscopy (LabRAM, HR Evolution), transmission electron microscopy (JEM-2010 Plus, JEOL), scanning electron microscopy (SEM) (Hitachi, SU8230), and X-ray Diffraction (XRD) (D8 Advance, Bruker, Germany) using CuKα radiation (1.5406 Å) at 40 kV and 40 mA. Fourier transform infrared (FTIR) spectroscopy was used to characterize the chemical structures of the GP and GPD materials using a Nicolet iS50 (Thermo Scientific, USA). The thermal properties of the prepared composite films were examined by differential scanning calorimetry (DSC 3+, Mettler Toledo, Switzerland) under a nitrogen atmosphere (flow rate of 60 mL/min) and a heating/cooling rate of 10 °C/min.

The printed samples were subjected to tensile testing using a universal testing machine (T-series, model H5TK, Tinius Olsen, UK) equipped with a 1000 N load cell at a speed of 50 mm/min, in accordance with ASTM D882. The surface wettability of the samples was assessed using the water contact angle (WCA) at room temperature by dropping DI water onto the composite films. The droplet image was recorded with a Dino-Lite digital microscope (AM4815ZT, Taiwan), and its WCA was determined using ImageJ. The electrical conductivity of the composite films was measured using a standard two-probe method with a multimeter (Keithley DMM 6500) in accordance with ASTM D257 for DC resistance or conductance of insulating materials. The electrical conductivity of the composite samples was calculated as

ρ=1RsPG×t 1

where ρ is electrical conductivity (S.cm–1), Rs is the measured resistance (Ω), t is the specimen thickness (cm), P is the specimen width (cm), and G is the distance between the electrodes in the fixture (cm).

3. Results and Discussion

3.1. Structural Analysis of the GP and GPD Samples

The synthesized GP structures were characterized by Raman spectroscopy, as shown in Figure a. GP exhibited distinct features compared with GH. GH exhibited the characteristic D, G, and 2D bands at approximately 1342, 1571, and 2691 cm–1, respectively, with a relatively weak D band characteristic of its highly ordered graphitic structure. In comparison, GP exhibited a well-defined G band at approximately 1565 cm–1 and a 2D band at approximately 2686 cm–1, along with a more pronounced, broadened D band centered at approximately 1345 cm–1. The G-band shift from 1571 cm–1 for GH to 1565 cm–1 for GP suggests a change in the electronic environment of the graphitic structure, corresponding to an estimated Fermi-level shift of approximately 0.14 eV. , The I D /I G ratio increased from 0.15 for GH to 0.38 for GP, indicating an increase in Raman-active defects and/or exposed edge sites following exfoliation. This increase can be attributed to the electrolytic exfoliation process, during which the electric field facilitates the interaction and intercalation of sulfonate anions within the graphite structure, disrupting the ordered stacking and generating additional edge and defect sites. − Nevertheless, the I D /I G value of 0.38 remains considerably lower than values exceeding unity commonly reported for strongly defective chemically derived graphene, suggesting that the electrolytic exfoliation process largely preserves the sp2-bonded carbon framework. , Using the Cançado relationship with a 532 nm excitation wavelength, the I D /I G values correspond to a reduction in the Raman-derived lateral graphitic domain size (L a ) from approximately 128 nm for GH to 51 nm for GP, consistent with the generation of smaller graphitic domains and additional edge sites during exfoliation.

2.

2

(a) Raman spectra of the GP and pristine GH, (b) XRD pattern and TEM images of (c) the GP, and (d) a detailed view of the GP in the edge plane area, respectively.

To further investigate the out-of-plane crystalline structure and interlayer stacking of GP, XRD analysis was performed (Figure b). Pristine GH exhibited an intense (002) diffraction peak at 2θ = 26.45°, together with the second-order (004) reflection at 54.46°, characteristic of crystalline graphite. , GP retained these characteristic graphitic reflections but exhibited broader and less intense diffraction peaks, indicating decreased long-range stacking order and reduced coherent crystallite dimensions following exfoliation. , The (002) reflection shifted slightly from 26.45° for GH to 26.39° for GP, corresponding to a slight increase in the interlayer spacing, d002, from approximately 0.337 to 0.338 nm. Concurrently, the fwhm of the (002) reflection increased from 0.345 to 0.359°, indicating a reduction in the coherent crystallite thickness along the c-axis.

Using the Scherrer equation, the average crystallite thickness (L c ) decreased from approximately 23.4 nm for GH to 22.5 nm for GP. Based on the corresponding d002 values, these dimensions are equivalent to approximately 69 and 67 coherently stacked graphitic layers, respectively. It should be emphasized that these values represent the number of layers within an X-ray coherent stacking domain rather than the total number of graphene layers in an individual particle. The decrease in L c , together with the broadening and reduced intensity of the (002) reflection and the slight increase in d002, demonstrates partial disruption of the ordered graphite stacking during electrolytic exfoliation. These XRD results complement the Raman observations: the increase in I D /I G and corresponding reduction in L a indicate smaller in-plane graphitic domains and increased edge/defect density, whereas the increase in I 2D /I G indicates weakened interlayer coupling. Collectively, the Raman, XRD, and TEM results demonstrate that electrolytic exfoliation partially delaminates the graphite structure while largely preserving the sp2-bonded carbon framework, yielding multilayer graphene with reduced stacking order and increased accessible edge sites.

The morphology and microstructures of GP and its derivatives after modification with AKD at various concentrations were characterized by FESEM, as shown in Figure . The synthesized GP (Figure a) exhibited an average microscale particle size and was characterized by irregular, relatively large grains. Upon mechanical ball milling with AKD, a clear trend of size reduction was observed. The average GPD size decreased with increasing AKD content, indicating that milling effectively fractured larger particles (Figure a–e). However, when the AKD content reached 30 wt %, particle accumulation and agglomeration became increasingly prominent (Figure f). It resembled the morphology of GPD0 (without AKD) and the original GP. This phenomenon can be attributed to the inherent waxy characteristics and low melting point (50 °C) of AKD. The AKD pellets likely melted and served as a lubricant during ball milling. At lower AKD concentrations (exceeding 20 wt %), the melted AKD appeared to form a hydrophobic coating on the graphene sheets. While it potentially aids dispersion in nonpolar matrices, it promotes the reagglomeration of GP particles (at 30 wt %), leading to larger particle sizes and accumulation. Therefore, GPD20 was selected as the optimal composite for subsequent experiments, as it plays a key role in its good dispersion within the PLA polymer matrix.

3.

3

SEM micrographs of GP after modification via ball milling with various concentrations of AKD: (a) neat GP, (b) GPD0, (c) GPD5, (d) GPD10, (e) GPD20, and (f) GPD30.

The chemical composition and interactions within GP and GPD were investigated using FTIR spectroscopy, as displayed in Figure . The prepared GP spectrum served as a baseline. The GPD5 and GPD10 spectra did not exhibit distinct bands, indicating that the amount of AKD was below the technique’s detection limit. In contrast, GPD20 and GPD30 showed weak new bands at approximately 2919 and 2851 cm–1 for GPD20 and 2925 and 2855 cm–1 for GPD30, respectively. These bands are similar to the prominent bands observed in neat AKD at 2914 and 2847 cm–1, which are attributed to C–H vibrations of the methylene (−CH2) and methyl (−CH3) groups of the long alkyl chains present in the AKD molecule. , The appearance of these major bands in GPD20 and GPD30 confirms the successful incorporation of AKD into the GP sheets at the specified concentrations during the ball-milling modification process.

4.

4

FTIR spectra of (a) GP and modified GP with various AKD concentrations through a ball milling process: (b) GPD5, (c) GPD10, (d) GPD20, (e) GPD30, and (f) neat AKD.

Ball milling may promote interactions between the hydroxyl groups on the GP surface and the highly reactive ketene-dimer functionality of AKD. Formation of β-keto ester linkages through covalent reactions would be expected to generate characteristic absorption bands in the 1750–1700 cm–1 region. , However, this spectral region overlaps with bands originating from GP, making definitive identification of such covalent bonding difficult based solely on FTIR analysis. Therefore, while the FTIR results provide evidence of AKD on the GP surface, they do not conclusively distinguish covalent attachment from physical adsorption or other interfacial interactions. Consequently, the modified graphene is considered to contain AKD associated with the GP surface through a combination of possible covalent bonding and physical interfacial interactions.

3.2. Biomaterial Composite Films

3.2.1. FTIR Analysis of the PLA Film and Its Composites

In Figure , the FTIR spectra of all samples exhibited characteristic bands within the 3000–2850 cm–1 region, which are ascribed to the C–H stretching vibrations of the methine and methyl groups inherent to the PLA structure. A key observation in the PLA-GPD20 composite films, particularly compared with neat PLA, is the presence of bands at 2914 and 2847 cm–1. These bands are attributed to the C–H vibrations of the methylene and methyl groups within the long alkyl chains of the incorporated AKD. , In addition, the intensity of the AKD-specific bands increased progressively with higher concentrations of GPD20 incorporated into the composite films, providing clear evidence of successful AKD incorporation within the PLA matrix.

5.

5

FTIR spectra of: (a) neat PLA and PLA/GPD20 composites with GPD20 at various compositions: (b) 5%, (c) 10%, (d) 15%, (e) 20%, and (f) 30%.

The FTIR spectra also revealed a prominent carbonyl (CO) stretching band, which appeared as a split signal at 1755 and 1746 cm–1. This splitting is well established as indicative of the distinct crystalline and amorphous phases within the PLA component, and is consistent with previous studies on PLA crystallinity. − There are other relevant signals, such as the band around 1200 cm–1, assigned to the asymmetric −C–O-C stretching modes, which are linked to asymmetric −CH3 rocking vibrations and also split into two bands at 1210 and 1179 cm–1. , Notably, all samples showed a band around 920 cm–1, a characteristic of the α-crystal band of PLA, arising from the −CH3 rocking mode of α crystals. The absorption bands at 868 and 753 cm–1 are further related to the C–C stretching vibrations and correspond to the amorphous and crystalline phases of PLA, respectively. However, the FTIR spectra did not show peaks of GP, indicating that PLA is sensitive to IR rays, which cover the weak GP bands.

To examine the structural characteristics of GPD20 and its interactions with the PLA matrix, Raman spectroscopy was performed, as shown in Figure . Neat PLA exhibited characteristic Raman bands at 2998 and 2943 cm–1, corresponding to the C–H stretching vibrations of the −CH3 groups. The bands at approximately 1450 and 870 cm–1 are assigned to C–H deformation and stretching of the C–COO units, respectively, while the weak band at approximately 1775 cm–1 is attributed to the CO stretching mode of the ester groups in PLA. GPD20 exhibited the characteristic graphitic D, G, and 2D bands at 1355, 1590, and 2700 cm–1, respectively. Relative to GP, the G and 2D bands of GPD20 shifted toward higher wavenumbers (ΔωG = +25 cm–1 and Δω2D = +14 cm–1), yielding a Δω2D/ΔωG ratio of approximately 0.56. These shifts indicate changes in the local electronic and strain environment of the graphene sheets following AKD modification and are consistent with perturbation of the graphitic structure. ,

6.

6

Raman spectra of (a) neat PLA, (b) PLA/GPD20-10% composite, and (c) GPD20 products.

Quantitative analysis using the same baseline-correction procedure showed that the I D /I G ratio increased from approximately 0.38 for GP to 0.48 for GPD20. For a Raman excitation wavelength of 532 nm, the corresponding lateral graphitic domain size (L a ), calculated using the Cançado relationship, decreased from approximately 51 to 40 nm. The increase in I D /I G and decrease in L a indicate an increase in Raman-active defects and/or exposed edge sites following modification. This behavior may arise from further delamination and fragmentation of the graphene sheets during the modification process, as well as from local structural perturbations induced by the modifier. Importantly, this increase in D-band intensity does not necessarily indicate extensive destruction of the sp2-carbon framework, as exfoliation itself increases the density of exposed graphene edges, contributing to the D band.

More pronounced structural changes were observed in the 2D band. The I D /I G ratio increased substantially from 0.52 for GP to 1.39 for GPD20, indicating weakened interlayer coupling and a substantially greater degree of graphene delamination following modification. Although an I D /I G ratio greater than unity is generally associated with relatively thin graphene structures, the intensity ratio alone cannot be used to assign an exact number of graphene layers, particularly for chemically modified graphene. Therefore, rather than assigning GPD20 specifically as bilayer graphene, the Raman results indicate that GPD20 possesses a more highly exfoliated and less strongly coupled graphitic structure than GP.

Following incorporation of GPD20 into the PLA matrix, the characteristic graphene D, G, and 2D bands were observed at approximately 1350, 1585, and 2720 cm–1, respectively. The shifts in the G and 2D bands relative to those of GPD20 indicate changes in the local electronic and/or strain environment of graphene upon incorporation into PLA, supporting interactions between the modified graphene surface and the polymer matrix. Such interactions may involve the π-electron system of graphene and the polar ester groups of PLA, as well as those associated with AKD-derived surface functionalities. The I D /I G ratio remained relatively unchanged at approximately 0.49, corresponding to an L a of approximately 39 nm, suggesting that the lateral graphitic domain structure of GPD20 was largely retained after composite processing.

In contrast, the I 2D /I G ratio decreased markedly from approximately 1.39 for GPD20 to 0.43 for PLA/GPD20-10%. This decrease indicates increased interlayer coupling and may reflect partial reassociation or restacking of the exfoliated graphene sheets during composite fabrication. However, changes in graphene orientation, the local dielectric environment, polymer-graphene interactions, and contributions from the PLA Raman background may also affect the relative intensities of the 2D and G bands. Therefore, the decrease in I 2D /I G should not be interpreted solely in terms of the number of graphene layers. Nevertheless, the Raman results demonstrate that the modified graphene retains its relatively high edge/defect character after incorporation into PLA, while interactions with the polymer matrix and composite processing alter its interlayer organization. A weak broad band centered at 3250 cm–1 was also observed and may be assigned to O–H stretching vibrations. This feature may be associated with hydroxyl-containing species generated from hydrolysis or side reactions of the AKD modifier.

3.2.2. Thermal Properties of the Neat PLA and Composite Films

To investigate the effects of GPD20 content on the thermal properties of PLA/GPD20 composites, DSC thermograms were examined to evaluate their glass transition temperature (T g), melting temperature (T m), cold crystallization temperature (T c), and crystallinity (X c ) using the following equation:

Xc=(ΔHm−ΔHcΔHf×(1−wt.%100))×100 2

where ΔH m (J/g) represents the melting enthalpy of the sample, ΔH c (J/g) is the enthalpy of cold crystallization, ΔH f is the melt enthalpy (93.0 J/g) for 100% crystalline PLA, and wt % indicates the weight fraction of the total graphene in the PLA formulation. ,

DSC curves of the PLA and PLA-GPD20 composites from the first and second heating cycles are compared in Figure . The thermal characteristics and processing-induced history of the samples were explained by the initial DSC heating scans, which are mainly influenced by the preparation method (i.e., solvent casting). Figure a shows that neat PLA exhibited a T g at 41.8 °C and T m at 151.4 °C. The incorporation of GPD20, however, induced concentration-dependent modulation of these thermal transitions: T g initially increased to a maximum of 53.9 °C (PLA-GPD20-30), while Tm initially decreased slightly (142.8 °C) before rising, peaking at 146.1 °C for PLA-GPD20-10. This general trend of elevated T g and T m at higher GPD20 loadings is primarily attributed to the nucleating effect of GPD20. The presence of these nucleating sites restricts the segmental mobility of PLA chains, thereby requiring more energy for thermal transitions, a phenomenon consistent with previous literature. ,

7.

7

1st (a) and 2nd heating (b) DSC thermograms of neat PLA and PLA-GPD20 composite films at different GPD20 contents.

Interestingly, the second heating cycle (Figure b) revealed a noticeable shift in T g of PLA-GPD20 composites to lower temperatures compared to neat PLA. This behavior demonstrates that the polymer chain fragments in PLA-GPD20 composites are much more easily moved than those in the neat PLA matrix, perhaps because the filling of the composite sample decreased the entanglements of PLA chains. The T g transition also showed a sharp overshoot in the thermograms, indicating a physical aging phenomenon, particularly in the polymer composite films. Moreover, the T c peak for composite films (124.9–127.6 °C) shifted slightly to higher temperatures compared with neat PLA films (126.2 °C). It has been reported that this phenomenon is due to faster crystallization induced by fillers, which act as PLA polymer nucleating agents. Conversely, the T m of the PLA-GPD20 composites remained comparable to that of neat PLA, indicating that the overall crystalline phase was largely unaffected. In addition, as summarized in Table , incorporating GPD20 significantly affected the crystallinity of PLA in a nonmonotonic fashion during the first heating cycle; X c remarkably increased from 29.5% for neat PLA to 36.2% for PLA-GPD20-10 (corresponding to ΔHm = 30.5 J/g), strongly suggesting that AKD is an effective nucleating agent, likely through hydrogen bonding between its carbonyl groups and PLA. Beyond this optimal 10 wt % loading, X c values generally decreased, which, when coupled with the T g and T m shifts, indicates a complex interplay where AKD initially acts as both a nucleating agent and a plasticizer (easing chain motion for crystallization), but excessive GPD might induce aggregation or steric hindrance, counteracting these beneficial effects at higher concentrations. Similar complex, concentration-dependent behaviors in PLA composites have been reported elsewhere. ,

1. Thermal Properties of Neat PLA and PLA-GPD20 Composite Films at Different GPD20 Contents Derived from DSC Thermograms.
Samples GPD20 loading (wt %) Tg (°C) Tm (°C) ΔHm (J/g) Tc (°C) ΔHc (J/g) X c (%)
1st heating scan
Neat PLA 0.00 41.8 151.4 27.5 - - 29.5
PLA/GPD20-5 0.05 44.4 142.8 22.9 - - 25.8
PLA/GPD20-10 0.10 46.8 146.1 30.5 - - 36.2
PLA/GPD20-15 0.15 50.4 145.8 22.0 - - 27.7
PLA/GPD20-20 0.20 46.3 143.1 19.9 - - 26.6
PLA/GPD20-30 0.30 53.9 144.7 20.6 - - 31.4
2nd heating scan
Neat PLA 0.00 60.9 149.5 5.9 126.2 3.4 2.6
PLA/GPD20-5 0.05 57.4 150.6 0.9 126.2 0.4 0.6
PLA/GPD20-10 0.10 56.3 147.9 1.5 124.9 0.8 0.8
PLA/GPD20-15 0.15 57.2 148.9 1.6 127.6 1.0 0.8
PLA/GPD20-20 0.20 57.3 149.9 1.1 125.9 0.7 0.5
PLA/GPD20-30 0.30 57.7 150.2 1.5 127.2 0.9 0.9

3.2.3. Electrical Conductivity of PLA Composite Films

The electrical conductivity of the PLA-composite films was evaluated to substantiate the morphological observations. As a fundamental reference, neat PLA has negligible electrical conductivity, typically 10–6 S·cm–1, characteristic of polymeric insulators. Upon adding GPD20 at a content exceeding 20 wt %, a transition from nonconductivity to electrically conductive behavior was observed, marking the transition from an insulating to a conductive polymer. , The electrical conductivity values of the composite films increased to 22.60 × 10–6 and 332.31 × 10–6 S·cm–1 for those containing 20 and 30 wt % GPD20, respectively. This substantial improvement in electrical conductivity is likely attributable to the homogeneous distribution of GPD20, which progressively forms conductive pathways and enhances connectivity among GPD20 particles at higher filler loadings, thereby facilitating efficient electron transfer within the PLA matrix. However, the increase in electrical conductivity is more modest than that typically reported for graphene/polymer systems at comparable loadings. This is attributed to the presence of AKD, which simultaneously introduces a thin organic insulating layer at the GP surface. This layer likely increases intersheet contact resistance and partially impedes electron tunneling/hopping between adjacent graphene sheets. Nevertheless, these electrically conductive PLA-GPD20 composites are highly desirable for tissue engineering applications because they can provide essential electrical cues to support and significantly enhance the regeneration of electrically active tissues, such as nerve or cardiac tissues.

3.2.4. Mechanical Properties of Polylactic Acid and Its Composite Films

The mechanical properties of PLA and its composite films were characterized, and their stress–strain curves are shown in Figure . Neat PLA film exhibited the typical behavior of a brittle material, as indicated by its highest tensile strength of 44.1 ± 3.2 MPa, but concurrently the lowest elongation at break, measuring 2.9 ± 0.3%. The dense packing and strong intermolecular forces arising from numerous polar segments within its molecular chains, which restrict significant plastic deformation, are often linked to this inherent brittleness in neat PLA. In contrast, incorporating GPD20 into the PLA matrix significantly enhanced the elongation at break of the composite films. This improvement in ductility is largely due to the positive influence of AKD, which promotes the good dispersion of GPD20 within the PLA matrix and effectively contributes to the overall reinforcement and toughening mechanism. However, the tensile strengths of the composite films were consistently lower than that of the neat PLA film across all GPD20 loadings, even at high incorporation percentages (up to 30 wt %). This reduction in mechanical performance can be attributed to the presence of AKD, which may act as a plasticizer, enhancing the mobility of polymer chains and increasing interchain spacing within the PLA matrix. DSC results revealed both increased crystallinity and an elevated T g in the first heating scans, indicating restricted chain mobility and altered phase organization. However, such a restriction, coupled with reduced continuity of the amorphous phase and weakened interfacial adhesion between the PLA matrix and the GPD20 filler, likely hindered efficient stress transfer, resulting in premature tensile failure. This observation is consistent with previous studies showing that excessive nucleating or plasticizing additives can induce localized structural ordering while simultaneously diminishing the overall mechanical cohesion of semicrystalline polymers. ,,

8.

8

Mechanical properties of neat PLA and PLA-GPD20 composite films with different GPD20 compositions: (a) tensile stress–strain curves, (b) tensile strength, (c) Young’s modulus, and (d) elongation at break.

The PLA-GPD20 composites exhibited tensile strengths ranging from 33.5 ± 1.5 MPa (at 30 wt % GPD20) to 44.1 ± 3.2 MPa, and the Young’s modulus of 2,160 ± 215 MPa to 3,530 ± 221 MPa (at 15 wt % GPD20). As expected, the addition of GPD20 substantially improved the stiffness of the PLA matrix when incorporating a rigid filler, as evidenced by the significant increase in Young’s modulus. The highest modulus, achieved at 15 wt % GPD20, represents a substantial 63.4% enhancement compared with neat PLA. This marked increase in stiffness is primarily attributed to the intrinsically high modulus of graphene derivatives and their improved dispersibility within the polymer matrix, facilitated by the AKD modification step. Meanwhile, the elongation at break increased from 2.9 ± 0.3% for neat PLA to 4.8 ± 0.7% at 20 wt % GPD20 loading. This enhancement in ductility and toughness is primarily attributed to the effective surface modification of GPD20 using AKD. The presence of AKD effectively reduces unfavorable interfacial interactions between GPD20 and the PLA matrix, thereby promoting a more homogeneous dispersion of GPD20. , This improved interface minimizes stress concentration points and allows greater energy dissipation before fracture. Based on the overall mechanical performance, an optimal balance among stiffness, strength, and toughness was achieved at GPD20 contents of 10–20 wt %.

3.2.5. Surface Wettability

The surface wettability of neat PLA and its composites was determined through WCA measurements, as shown in Figure . Neat PLA film exhibited a typical hydrophilic behavior with a WCA of 75°, which agrees with previous work. , The incorporation of GPD20 into the PLA matrix increased the value to a range of 85–90°, reaching a maximum at 30 wt % GPD20 loading. This increased surface hydrophobicity is primarily attributed to AKD migration to the composite film surfaces. , This is supported by the ATR-FTIR results, in which the characteristic bands of AKD’s long alkyl chains became prominent. The presence of AKD enhanced the compatibility of GPD20 in the PLA matrix and significantly improved the surface hydrophobicity of the composite films.

9.

9

Water contact angle (WCA) value of neat PLA and its composite films with different GPD20 compositions.

3.3. Evaluation of the Potential Applications of 3D-Printed PLA-GPD20 Composites

Compared with neat PLA, the PLA composite containing 10 wt % GPD20 was chosen as the optimal material for fabricating scaffold samples via 3D bioprinting, as it provides the best balance among the relevant properties, i.e., conductivity, ductility, strength, printability, and crystallinity. The properties and performances of the printed specimens were evaluated for potential scaffold applications. The two materials were printed with two distinct pattern orientations (45° and 90° relative to the tensile direction) to investigate the influence of printing direction, a particularly relevant parameter for tissue engineering applications. Their mechanical performance was assessed by tensile testing, with the stress–strain curves compared in Figure a, and Table summarizes the corresponding mechanical properties. Substantial improvements in tensile strength and Young’s modulus were observed after adding 10 wt % GPD20. For the 45° printing orientation, the tensile strength increased from 5.31 ± 0.21 MPa (Neat PLA-45°) to 6.20 ± 0.55 MPa (10%–45°), and the Young’s modulus increased from 137 ± 6 MPa to 164 ± 17 MPa. Similarly, for the 90° orientation, the tensile strength increased from 3.30 ± 0.51 MPa (Neat PLA-90°) to 4.58 ± 0.23 MPa (10%–90°), and the Young’s modulus increased from 158 ± 18 MPa to 308 ± 31 MPa. This is likely because GPD20 acts as a strong, well-dispersed phase that effectively stiffens the composite, facilitating efficient stress transfer to the GPD20 domains. The role of GPD20 as a reinforcing filler for PLA scaffolds is further evidenced by a general decrease in elongation at break in the composites compared to their pure PLA counterparts, indicating an enhancement in overall material stiffness.

10.

10

(a) Stress and strain curves of neat PLA and PLA-GPD20–10 composite scaffolds, printed at (b) 90° and (c) 45° patterns, after tensile testing.

2. Mechanical Properties of Neat PLA and Its PLA-GPD20-10 Composite Scaffolds Printed at Different Orientation Patterns.

Samples Elongation at the yield (%) Elongation at break (%) Tensile strength (MPa) Young’s modulus (MPa)
Neat PLA-45° 6.73 ± 0.24 62.80 ± 6.00 5.31 ± 0.21 137 ± 5.97
PLA-GPD20–10 −45° 8.68 ± 0.10 61.0 ± 6.30 6.20 ± 0.55 164 ± 17.50
Neat PLA-90° 3.80 ± 0.10 139.0 ± 5.56 3.30 ± 0.51 158 ± 18.03
PLA-GPD20–10 −90° 3.52 ± 0.10 24.5 ± 0.24 4.58 ± 0.23 308 ± 31.40

Regarding the influence of printing orientation, the scaffold printed with a 90° orientation exhibited significantly higher Young’s modulus than the scaffold oriented at 45°. Specifically, the PLA-GPD20–10–90° sample had a Young’s modulus of 308 ± 31 MPa, whereas the PLA-GPD20–10–45° sample showed 164 ± 17 MPa. This difference is explained by the alignment of the applied tensile force with the printing raster orientation in the 90° sample, resulting in more effective load bearing and stretching directly along the scaffold structure. , This behavior is visualized in the fracture patterns shown in Figure b and c for the 45° pattern, illustrating distinct failure modes depending on orientation.

In terms of mechanical deformation, the elongation at yield, which marks the end of the elastic region and the onset of plastic deformation, also varied with orientation. The 45° samples (both neat and composite) generally exhibited larger elongation at yield values than the 90° samples (e.g., 8.68 ± 0.10% for PLA-GPD20–10–45° vs. 3.52 ± 0.10% for PLA-GPD20–10–90°). This behavior can be attributed to the orientation of the printed pattern: in 45° samples, a portion of the applied stress is initially used to deform and reorient the scaffold structure itself, allowing for greater initial elongation. Conversely, the stress is applied more directly along the fiber direction in the 90° samples, resulting in less initial elastic deformation. Overall, the consistent diminishing of elongation at break upon adding GPD20 filler to PLA scaffolds, across both orientations, underscores GPD20s effective role as a reinforcing agent that significantly enhances the composite material’s stiffness.

4. Conclusions

This study successfully developed and characterized novel multifunctional biomaterial inks based on AKD-modified graphene nanoplatelets (GPD20) incorporated into a PLA biopolymer for extrusion-based 3D bioprinting of complex scaffolds. Characterization confirmed the preparation of GPD20 via electrolytic exfoliation of graphene and AKD modification through ball milling, which was crucial for enhancing dispersion and compatibility with the PLA matrix. The FTIR analysis provided clear evidence of AKD incorporation into GPD20 and its presence within the PLA-GPD20 composites. The evaluation of the PLA-GPD20 films revealed several key improvements in the material properties. While a slight decrease in overall tensile strength was observed in the composite films compared to neat PLA, the incorporation of GPD20 significantly enhanced the elongation at break, increasing from 2.9 ± 0.3% for neat PLA to a peak of 4.8 ± 0.7% at 20 wt % GPD20, indicating improved ductility and toughness.

Furthermore, GPD20 acted as an effective reinforcing filler, significantly enhancing the mechanical properties of the PLA matrix. The Young’s modulus increased by up to 63.4% at a GPD20 loading of 15 wt %, while an optimal balance of stiffness, strength, processability, and other functional properties was achieved within the 10–20 wt % GPD20 range. Regarding surface wettability, the composites exhibited increased hydrophobicity, with the water contact angle increasing from approximately 75° for neat PLA to nearly 90° for the GPD20-containing composites. This behavior was primarily attributed to the presence and migration of AKD-derived hydrophobic alkyl chains at the film surface. In terms of thermal properties, GPD20 acted as a nucleating agent, promoting PLA crystallization without significantly altering T g or T m. The highest crystallinity was observed at 10 wt % GPD20, increasing from 29.5% for neat PLA to 36.2%. The PLA/GPD20 composites also exhibited a substantial increase in electrical conductivity at GPD20 loadings above 20 wt %, reaching 332.31 × 10–6 S·cm–1 at 30 wt %. This enhancement is attributed to the formation of conductive pathways through improved connectivity among graphene particles at higher filler contents, making these materials attractive candidates for applications requiring electrically responsive properties. The incorporation of 10 wt % GPD20 was selected for scaffold fabrication because it provided the most favorable balance of mechanical performance, crystallinity, printability, and filler dispersion. The resulting scaffolds exhibited significantly improved tensile strength and Young’s modulus compared with neat PLA scaffolds. In addition, the orientation of the printing pattern strongly influenced the mechanical behavior of the scaffolds, demonstrating that stiffness and ductility can be tailored through printing design. Scaffolds printed with a 90° raster orientation exhibited a higher Young’s modulus, whereas those printed with a 45° orientation showed greater tensile strength and elongation at yield. These differences were attributed to variations in load transfer and filament alignment relative to the applied tensile force.

This research demonstrates that AKD-modified graphene composites, which leverage AKD’s ability to improve graphene dispersion, enhance compatibility with the PLA matrix, promote PLA crystallization, and modify surface properties, are promising materials for fabricating multifunctional 3D-printed scaffolds. The ability to tailor mechanical performance, surface wettability, and electrical conductivity, together with excellent printability and the capability to tune scaffold properties through printing orientation, provides a versatile platform for the development of advanced scaffold materials. These findings highlight the potential of the developed composites for tissue engineering applications. However, their biological performance has not yet been evaluated. Future studies will focus on assessing cytocompatibility, cell adhesion, proliferation, and biodegradation behavior to establish their suitability for specific tissue engineering applications.

Acknowledgments

The authors gratefully acknowledge financial support from the Thailand Science Research and Innovation Fundamental Fund Fiscal Year 2570, and the Center of Excellence in Functional Advanced Materials Engineering (CoE FAME), Thammasat University. The facility support provided from the Thailand Organic & Printed Electronics Innovation Center (TOPIC) is gratefully acknowledged. W.K. gratefully acknowledges the SIIT Faculty’s Quota Scholarship from SIIT, Thammasat University. Part of this work was presented at the POLY-CHAR 2026 Conference, held in Chiang Mai, Thailand.

The authors declare no competing financial interest.

References

  1. Sindhi K., Pingili R. B., Beldar V., Bhattacharya S., Rahaman J., Mukherjee D.. The role of biomaterials-based scaffolds in advancing skin tissue construct. J. Tissue Viability. 2025;34:100858. doi: 10.1016/j.jtv.2025.100858. [DOI] [PubMed] [Google Scholar]
  2. Kaniuk Ł., Stachewicz U.. Development and advantages of biodegradable PHA polymers based on electrospun PHBV fibers for tissue engineering and other biomedical applications. ACS Biomater. Sci. Eng. 2021;7(12):5339–5362. doi: 10.1021/acsbiomaterials.1c00757. [DOI] [PMC free article] [PubMed] [Google Scholar]
  3. Nokoorani Y. D., Shamloo A., Bahadoran M., Moravvej H.. Fabrication and characterization of scaffolds containing different amounts of allantoin for skin tissue engineering. Sci. Rep. 2021;11(1):16164. doi: 10.1038/s41598-021-95763-4. [DOI] [PMC free article] [PubMed] [Google Scholar]
  4. Agarwal S., Saha S., Balla V. K., Pal A., Barui A., Bodhak S.. Current developments in 3D bioprinting for tissue and organ regeneration–a review. Front. Mech. Eng. 2020;6:589171. doi: 10.3389/fmech.2020.589171. [DOI] [Google Scholar]
  5. Agarwala S.. A perspective on 3D bioprinting technology: Present and future. Am. J. Eng. Applied Sci. 2016;9:985–990. doi: 10.3844/ajeassp.2016.985.990. [DOI] [Google Scholar]
  6. Abdelaziz A. G., Nageh H., Abdo S. M., Abdalla M. S., Amer A. A., Abdal-Hay A., Barhoum A.. A review of 3D polymeric scaffolds for bone tissue engineering: principles, fabrication techniques, immunomodulatory roles, and challenges. Bioengineering. 2023;10(2):204. doi: 10.3390/bioengineering10020204. [DOI] [PMC free article] [PubMed] [Google Scholar]
  7. Ashammakhi N., Ahadian S., Xu C., Montazerian H., Ko H., Nasiri R., Barros N., Khademhosseini A.. Bioinks and bioprinting technologies to make heterogeneous and biomimetic tissue constructs. Mater. Today Bio. 2019;1:100008. doi: 10.1016/j.mtbio.2019.100008. [DOI] [PMC free article] [PubMed] [Google Scholar]
  8. Liu S., Qin S., He M., Zhou D., Qin Q., Wang H.. Current applications of poly (lactic acid) composites in tissue engineering and drug delivery. Composites, Part B. 2020;199:108238. doi: 10.1016/j.compositesb.2020.108238. [DOI] [Google Scholar]
  9. Gangolphe L., Leon-Valdivieso C. Y., Nottelet B., Déjean S., Bethry A., Pinese C., Bossard F., Garric X.. Electrospun microstructured PLA-based scaffolds featuring relevant anisotropic, mechanical and degradation characteristics for soft tissue engineering. Mater. Sci. Eng. 2021;129:112339. doi: 10.1016/j.msec.2021.112339. [DOI] [PubMed] [Google Scholar]
  10. Kirillova A., Yeazel T. R., Asheghali D., Petersen S. R., Dort S., Gall K., Becker M. L.. Fabrication of biomedical scaffolds using biodegradable polymers. Chem. Rev. 2021;121(18):11238–11304. doi: 10.1021/acs.chemrev.0c01200. [DOI] [PubMed] [Google Scholar]
  11. Fattahi F. S., Khoddami A., Avinc O.. Poly (lactic acid)­(PLA) nanofibers for bone tissue engineering. J. Textiles Polym. 2019;7(2):47–64. [Google Scholar]
  12. Torres E., Gaona A., García-Bosch N., Muñoz M., Fombuena V., Moriana R., Vallés-Lluch A.. Improved mechanical, thermal, and hydrophobic properties of PLA modified with alkoxysilanes by reactive extrusion process. Polymers. 2021;13(15):2475. doi: 10.3390/polym13152475. [DOI] [PMC free article] [PubMed] [Google Scholar]
  13. Zhao X., Yu J., Liang X., Huang Z., Li J., Peng S.. Crystallization behaviors regulations and mechanical performances enhancement approaches of polylactic acid (PLA) biodegradable materials modified by organic nucleating agents. Int. J. Biol. Macromol. 2023;233:123581. doi: 10.1016/j.ijbiomac.2023.123581. [DOI] [PubMed] [Google Scholar]
  14. Huo X., Wan P., Zhang R., Zhang Z., Lv S.. Enhancing the strength and toughness of polylactic acid-based composites through one-step co-deposition of active coating onto wood fiber. Int. J. Biol. Macromol. 2024;274:133414. doi: 10.1016/j.ijbiomac.2024.133414. [DOI] [PubMed] [Google Scholar]
  15. Ho M.-P., Lau K.-T., Wang H., Hui D.. Improvement on the properties of polylactic acid (PLA) using bamboo charcoal particles. Composites, Part B. 2015;81:14–25. doi: 10.1016/j.compositesb.2015.05.048. [DOI] [Google Scholar]
  16. Ajaj Y., Al-Salman H. N. K., Hussein A. M., Jamee M. K., Abdullaev S., Omran A. A., Karim M. M., Abdulwahid A. S., Mahmoud Z. H., Kianfar E.. Effect and investigating of graphene nanoparticles on mechanical, physical properties of polylactic acid polymer. Case Stud. Chem. Environ. Eng. 2024;9:100612. doi: 10.1016/j.cscee.2024.100612. [DOI] [Google Scholar]
  17. Cruz R., Nisar M., Palza H., Yazdani-Pedram M., Aguilar-Bolados H., Quijada R.. Development of bio degradable nanocomposites based on PLA and functionalized graphene oxide. Polym. Test. 2023;124:108066. doi: 10.1016/j.polymertesting.2023.108066. [DOI] [Google Scholar]
  18. Chen Y., Yao X., Zhou X., Pan Z., Gu Q.. Poly (lactic acid)/graphene nanocomposites prepared via solution blending using chloroform as a mutual solvent. J. Nanosci. Nanotechnol. 2011;11(9):7813–7819. doi: 10.1166/jnn.2011.4732. [DOI] [PubMed] [Google Scholar]
  19. Marouazi H. E., Schueren B. V. D., Favier D., Bolley A., Dagorne S., Dintzer T., Janowska I.. Great enhancement of mechanical features in PLA based composites containing aligned few layer graphene (FLG), the effect of FLG loading, size, and dispersion on mechanical and thermal properties. J. Appl. Polym. Sci. 2021;138(44):51300. doi: 10.1002/app.51300. [DOI] [Google Scholar]
  20. Seok J. M., Choe G., Lee S. J., Yoon M.-A., Kim K.-S., Lee J. H., Kim W. D., Lee J. Y., Lee K., Park S. A.. Enhanced three-dimensional printing scaffold for osteogenesis using a mussel-inspired graphene oxide coating. Mater. Des. 2021;209:109941. doi: 10.1016/j.matdes.2021.109941. [DOI] [Google Scholar]
  21. Kumar S., Chatterjee K.. Comprehensive Review on the Use of Graphene-Based Substrates for Regenerative Medicine and Biomedical Devices. ACS Appl. Mater. Interfaces. 2016;8(40):26431–26457. doi: 10.1021/acsami.6b09801. [DOI] [PubMed] [Google Scholar]
  22. Gerdefaramarzi R. S., Ebrahimian-Hosseinabadi M., Khodaei M.. 3D printed poly (lactic acid)/poly (ε-caprolactone)/graphene nanocomposite scaffolds for peripheral nerve tissue engineering. Arabian J. Chem. 2024;17(9):105927. doi: 10.1016/j.arabjc.2024.105927. [DOI] [Google Scholar]
  23. Seyedsalehi A., Daneshmandi L., Barajaa M., Riordan J., Laurencin C. T.. Fabrication and characterization of mechanically competent 3D printed polycaprolactone-reduced graphene oxide scaffolds. Sci. Rep. 2020;10(1):22210. doi: 10.1038/s41598-020-78977-w. [DOI] [PMC free article] [PubMed] [Google Scholar]
  24. Tang L.-C., Wan Y.-J., Yan D., Pei Y.-B., Zhao L., Li Y.-B., Wu L.-B., Jiang J.-X., Lai G.-Q.. The effect of graphene dispersion on the mechanical properties of graphene/epoxy composites. Carbon. 2013;60:16–27. doi: 10.1016/j.carbon.2013.03.050. [DOI] [Google Scholar]
  25. Vasileiou A. A., Kontopoulou M., Docoslis A.. A noncovalent compatibilization approach to improve the filler dispersion and properties of polyethylene/graphene composites. ACS Appl. Mater. Interfaces. 2014;6(3):1916–1925. doi: 10.1021/am404979g. [DOI] [PubMed] [Google Scholar]
  26. Zhang K., Mao L., Zhang L. L., Chan H. S. O., Zhao X. S., Wu J.. Surfactant-intercalated, chemically reduced graphene oxide for high performance supercapacitor electrodes. J. Mater. Chem. 2011;21(20):7302–7307. doi: 10.1039/c1jm00007a. [DOI] [Google Scholar]
  27. Guardia L., Fernández-Merino M., Paredes J., Solís-Fernández P., Villar-Rodil S., Martínez-Alonso A., Tascón J.. High-throughput production of pristine graphene in an aqueous dispersion assisted by non-ionic surfactants. Carbon. 2011;49(5):1653–1662. doi: 10.1016/j.carbon.2010.12.049. [DOI] [Google Scholar]
  28. Huang K., Yu H., Xie M., Liu S., Wu F.. Effects of poly (ethylene glycol)-grafted graphene on the electrical properties of poly (lactic acid) nanocomposites. RSC Adv. 2019;9(19):10599–10605. doi: 10.1039/C9RA01060B. [DOI] [PMC free article] [PubMed] [Google Scholar]
  29. Lage-Rivera S., Ares-Pernas A., Becerra Permuy J. C., Gosset A., Abad M.-J.. Enhancement of 3D printability by FDM and electrical conductivity of PLA/MWCNT filaments using lignin as bio-dispersant. Polymers. 2023;15(4):999. doi: 10.3390/polym15040999. [DOI] [PMC free article] [PubMed] [Google Scholar]
  30. Wang M., Deng X.-Y., Du A.-K., Zhao T.-H., Zeng J.-B.. Poly (sodium 4-styrenesulfonate) modified graphene for reinforced biodegradable poly (ε-caprolactone) nanocomposites. RSC Adv. 2015;5(89):73146–73154. doi: 10.1039/C5RA15252F. [DOI] [Google Scholar]
  31. Lu J. Z., Wu Q., McNabb H. S.. Chemical coupling in wood fiber and polymer composites: A review of coupling agents and treatments. Wood Fiber Sci. 2000;32:88–104. [Google Scholar]
  32. Chartarrayawadee W., Molloy R., Ratchawet A., Janmee N., Butsamran M., Panpai K.. Fabrication of poly (lactic acid)/graphene oxide/stearic acid composites with improved tensile strength. Polym. Compos. 2017;38(10):2272–2282. doi: 10.1002/pc.23809. [DOI] [Google Scholar]
  33. Karuwan C., Wisitsoraat A., Phokharatkul D., Sriprachuabwong C., Lomas T., Nacapricha D., Tuantranont A.. A disposable screen printed graphene–carbon paste electrode and its application in electrochemical sensing. RSC Adv. 2013;3(48):25792–25799. doi: 10.1039/c3ra44187c. [DOI] [Google Scholar]
  34. Sriprachuabwong C., Duangsripat S., Sajjaanantakul K., Wisitsoraat A., Tuantranont A.. Electrolytically exfoliated graphene–polylactide-based Bioplastic with high elastic performance. J. Appl. Polym. Sci. 2015;132(6):41439. doi: 10.1002/app.41439. [DOI] [Google Scholar]
  35. Szroeder P., Banaszak-Piechowska A., Sahalianov I.. Tailoring Electrocatalytic Properties of sp2-Bonded Carbon Nanoforms Through Doping. Molecules. 2025;30(6):1265. doi: 10.3390/molecules30061265. [DOI] [PMC free article] [PubMed] [Google Scholar]
  36. Froehlicher G., Berciaud S.. Raman spectroscopy of electrochemically gated graphene transistors: Geometrical capacitance, electron-phonon, electron-electron, and electron-defect scattering. Phys. Rev. B. 2015;91(20):205413. doi: 10.1103/PhysRevB.91.205413. [DOI] [Google Scholar]
  37. Prakoso B., Ma Y., Stephanie R., Hawari N. H., Suendo V., Judawisastra H., Zong Y., Liu Z., Sumboja A.. Facile synthesis of battery waste-derived graphene for transparent and conductive film application by an electrochemical exfoliation method. RSC Adv. 2020;10(17):10322–10328. doi: 10.1039/D0RA01100B. [DOI] [PMC free article] [PubMed] [Google Scholar]
  38. Gorle D. B., Kumman V. V., Kulandainathan M. A.. Highly efficient, large surface area and spherically shaped Pt particles deposited electrolytically synthesized graphene for methanol oxidation with impedance spectroscopy. Int. J. Hydrogen Energy. 2017;42(25):16258–16268. doi: 10.1016/j.ijhydene.2017.05.160. [DOI] [Google Scholar]
  39. Wang G., Wang B., Park J., Wang Y., Sun B., Yao J.. Highly efficient and large-scale synthesis of graphene by electrolytic exfoliation. Carbon. 2009;47(14):3242–3246. doi: 10.1016/j.carbon.2009.07.040. [DOI] [Google Scholar]
  40. Singkammo S., Wisitsoraat A., Sriprachuabwong C., Tuantranont A., Phanichphant S., Liewhiran C.. Electrolytically Exfoliated Graphene-Loaded Flame-Made Ni-Doped SnO2 Composite Film for Acetone Sensing. ACS Appl. Mater. Interfaces. 2015;7(5):3077–3092. doi: 10.1021/acsami.5b00161. [DOI] [PubMed] [Google Scholar]
  41. Inyawilert K., Wisitsoraat A., Sriprachaubwong C., Tuantranont A., Phanichphant S., Liewhiran C.. Rapid ethanol sensor based on electrolytically-exfoliated graphene-loaded flame-made In-doped SnO2 composite film. Sens. Actuators, B. 2015;209:40–55. doi: 10.1016/j.snb.2014.11.086. [DOI] [PubMed] [Google Scholar]
  42. Hu M., Zhou Y., Nie W., Chen P.. Functionalized Graphene Nanosheets with Fewer Defects Prepared via Sodium Alginate Assisted Direct Exfoliation of Graphite in Aqueous Media for Lithium-Ion Batteries. ACS Appl. Nano Mater. 2018;1(4):1985–1994. doi: 10.1021/acsanm.8b00518. [DOI] [Google Scholar]
  43. Raj C. J., Manikandan R., Thondaiman P., Sivakumar P., Savariraj A. D., Cho W.-J., Kim B. C., Jung H.. Sonoelectrochemical exfoliation of graphene in various electrolytic environments and their structural and electrochemical properties. Carbon. 2021;184:266–276. doi: 10.1016/j.carbon.2021.08.027. [DOI] [Google Scholar]
  44. Cai W., Feng X., Hu W., Pan Y., Hu Y., Gong X.. Functionalized Graphene from Electrochemical Exfoliation for Thermoplastic Polyurethane: Thermal Stability, Mechanical Properties, and Flame Retardancy. Ind. Eng. Chem. Res. 2016;55(40):10681–10689. doi: 10.1021/acs.iecr.6b02579. [DOI] [Google Scholar]
  45. Sasrimuang S., Sirichat C., Puchongkawarin C., Jaiboon O., Luanwuthi S.. Environmentally Friendly Production of Graphene Oxide via Ball Milling: Characterization and Life Cycle Assessment. ACS Omega. 2025;10(28):30896–30905. doi: 10.1021/acsomega.5c03296. [DOI] [PMC free article] [PubMed] [Google Scholar]
  46. Karademir A.. Quantitative determination of alkyl ketene dimer (AKD) retention in paper made on a pilot paper machine. Turk. J. Agric. For. 2002;26(5):253–260. [Google Scholar]
  47. Caylak S., Ertas M., Donmez Cavdar A., Angin N.. Mechanical characteristics and hydrophobicity of alkyl ketene dimer compatibilized hybrid biopolymer composites. Polym. Compos. 2021;42(5):2324–2333. doi: 10.1002/pc.25980. [DOI] [Google Scholar]
  48. Angin N., Caylak S., Ertas M., Donmez Cavdar A.. Effect of alkyl ketene dimer on chemical and thermal properties of polylactic acid (PLA) hybrid composites. Sustainable Mater. Technol. 2022;32:e00386. doi: 10.1016/j.susmat.2021.e00386. [DOI] [Google Scholar]
  49. Cao H., Guo X., Zhou Y., Yan Y., Sun W.. Fabrication of Durable Hydrophobic/Superhydrophobic Wood Using an Alkyl Ketene Dimer by a Simple and Feasible Method. ACS Omega. 2022;7(21):17921–17928. doi: 10.1021/acsomega.2c01215. [DOI] [PMC free article] [PubMed] [Google Scholar]
  50. Eang C., Opaprakasit P.. Electrospun Nanofibers with Superhydrophobicity Derived from Degradable Polylactide for Oil/Water Separation Applications. J. Polym. Environ. 2020;28(5):1484–1491. doi: 10.1007/s10924-020-01704-z. [DOI] [Google Scholar]
  51. Ryu Y. S., Lee J. H., Kim S. H.. Efficacy of alkyl ketene dimer modified microcrystalline cellulose in polypropylene matrix. Polymer. 2020;196:122463. doi: 10.1016/j.polymer.2020.122463. [DOI] [Google Scholar]
  52. Nim B., Rahayu S. S., Thananukul K., Eang C., Opaprakasit M., Petchsuk A., Kaewsaneha C., Polpanich D., Opaprakasit P.. Sizing down and functionalizing polylactide (PLA) resin for synthesis of PLA-based polyurethanes for use in biomedical applications. Sci. Rep. 2023;13(1):2284. doi: 10.1038/s41598-023-29496-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
  53. Opaprakasit P., Opaprakasit M., Tangboriboonrat P.. Crystallization of Polylactide and Its Stereocomplex Investigated by Two-Dimensional Fourier Transform Infrared Correlation Spectroscopy Employing Carbonyl Overtones. Appl. Spectrosc. 2007;61(12):1352–1358. doi: 10.1366/000370207783292235. [DOI] [PubMed] [Google Scholar]
  54. Zhang J., Tsuji H., Noda I., Ozaki Y.. Structural Changes and Crystallization Dynamics of Poly­(l-lactide) during the Cold-Crystallization Process Investigated by Infrared and Two-Dimensional Infrared Correlation Spectroscopy. Macromolecules. 2004;37(17):6433–6439. doi: 10.1021/ma049288t. [DOI] [Google Scholar]
  55. Xing Q., Li R., Dong X., Luo F., Kuang X., Wang D., Zhang L.. Enhanced Crystallization Rate of Poly­(l-lactide) Mediated by a Hydrazide Compound: Nucleating Mechanism Study. Macromol. Chem. Phys. 2015;216(10):1134–1145. doi: 10.1002/macp.201500002. [DOI] [Google Scholar]
  56. Zhang H., Shao C., Kong W., Wang Y., Cao W., Liu C., Shen C.. Memory effect on the crystallization behavior of poly­(lactic acid) probed by infrared spectroscopy. Eur. Polym. J. 2017;91:376–385. doi: 10.1016/j.eurpolymj.2017.04.016. [DOI] [Google Scholar]
  57. Zhang J., Duan Y., Sato H., Tsuji H., Noda I., Yan S., Ozaki Y.. Crystal Modifications and Thermal Behavior of Poly­(l-lactic acid) Revealed by Infrared Spectroscopy. Macromolecules. 2005;38(19):8012–8021. doi: 10.1021/ma051232r. [DOI] [Google Scholar]
  58. Zhang C., Wang L., Zhai T., Wang X., Dan Y., Turng L.-S.. The surface grafting of graphene oxide with poly (ethylene glycol) as a reinforcement for poly (lactic acid) nanocomposite scaffolds for potential tissue engineering applications. J. Mechanical Behavior Biomed. Mater. 2016;53:403–413. doi: 10.1016/j.jmbbm.2015.08.043. [DOI] [PubMed] [Google Scholar]
  59. Liu S., Zheng Y., Wu Z., Hu J., Liu R.. Preparation and characterization of aspirin-loaded polylactic acid/graphene oxide biomimetic nanofibrous scaffolds. Polymer. 2020;211:123093. doi: 10.1016/j.polymer.2020.123093. [DOI] [Google Scholar]
  60. Li N., Wang M., Luo H., Tse S. D., Gao Y., Zhu Z., Guo H., He L., Zhu C., Yin K.. Processing and properties of graphene-reinforced polylactic acid nanocomposites for bioelectronic and tissue regenerative functions. Biomater Adv. 2025;167:214113. doi: 10.1016/j.bioadv.2024.214113. [DOI] [PubMed] [Google Scholar]
  61. Kim M., Jeong J. H., Lee J.-Y., Capasso A., Bonaccorso F., Kang S.-H., Lee Y.-K., Lee G.-H.. Electrically Conducting and Mechanically Strong Graphene–Polylactic Acid Composites for 3D Printing. ACS Appl. Mater. Interfaces. 2019;11(12):11841–11848. doi: 10.1021/acsami.9b03241. [DOI] [PubMed] [Google Scholar]
  62. Mueller N. S., Heeg S., Alvarez M. P., Kusch P., Wasserroth S., Clark N., Schedin F., Parthenios J., Papagelis K., Galiotis C.. Evaluating arbitrary strain configurations and doping in graphene with Raman spectroscopy. 2D Mater. 2018;5(1):015016. doi: 10.1088/2053-1583/aa90b3. [DOI] [Google Scholar]
  63. Keramati M., Ghasemi I., Karrabi M., Azizi H., Sabzi M.. Incorporation of surface modified graphene nanoplatelets for development of shape memory PLA nanocomposite. Fibers Polym. 2016;17(7):1062–1068. doi: 10.1007/s12221-016-6329-7. [DOI] [Google Scholar]
  64. Battegazzore D., Bocchini S., Frache A.. Crystallization kinetics of poly (lactic acid)-talc composites. Express Polym. Lett. 2011;5(10):849–858. doi: 10.3144/expresspolymlett.2011.84. [DOI] [Google Scholar]
  65. Valapa R. B., Pugazhenthi G., Katiyar V.. Effect of graphene content on the properties of poly (lactic acid) nanocomposites. RSC Adv. 2015;5(36):28410–28423. doi: 10.1039/C4RA15669B. [DOI] [Google Scholar]
  66. Kim S. W., Choi H. M.. Morphology, thermal, mechanical, and barrier properties of graphene oxide/poly (lactic acid) nanocomposite films. Korean J. Chem. Eng. 2016;33:330–336. doi: 10.1007/s11814-015-0142-7. [DOI] [Google Scholar]
  67. Wang L.-N., Guo Wang P.-Y., Wei J.-C.. Graphene oxide-graft-poly (l-lactide)/poly (l-lactide) nanocomposites: mechanical and thermal properties. Polymers. 2017;9(9):429. doi: 10.3390/polym9090429. [DOI] [PMC free article] [PubMed] [Google Scholar]
  68. Hernández Sánchez F., Molina Mateo J., Romero Colomer F. J., Salmerón Sánchez M., Gómez Ribelles J. L., Mano J. F.. Influence of Low-Temperature Nucleation on the Crystallization Process of Poly­(l-lactide) Biomacromolecules. 2005;6(6):3283–3290. doi: 10.1021/bm050323t. [DOI] [PubMed] [Google Scholar]
  69. Angin N., Caylak S., Ertas M., Cavdar A. D.. Effect of alkyl ketene dimer on chemical and thermal properties of polylactic acid (PLA) hybrid composites. Sustainable Mater. Technol. 2022;32:e00386. doi: 10.1016/j.susmat.2021.e00386. [DOI] [Google Scholar]
  70. Eang C., Nim B., Sreearunothai P., Petchsuk A., Opaprakasit P.. Chemical upcycling of polylactide (PLA) and its use in fabricating PLA-based super-hydrophobic and oleophilic electrospun nanofibers for oil absorption and oil/water separation. New J. Chem. 2022;46(31):14933–14943. doi: 10.1039/D2NJ02747J. [DOI] [Google Scholar]
  71. Yu W. W., Zhang J., Wu J. R., Wang X. Z., Deng Y. H.. Incorporation of graphitic nano-filler and poly­(lactic acid) in fused deposition modeling. J. Appl. Polym. Sci. 2017;134(15):44703. doi: 10.1002/app.44703. [DOI] [Google Scholar]
  72. Guo J., Tsou C.-H., Yu Y., Wu C.-S., Zhang X., Chen Z., Yang T., Ge F., Liu P., Guzman M. R. D.. Conductivity and mechanical properties of carbon black-reinforced poly (lactic acid)­(PLA/CB) composites. Iran. Polym. J. 2021;30(12):1251–1262. doi: 10.1007/s13726-021-00973-2. [DOI] [Google Scholar]
  73. Frąckowiak S., Kozlowski M.. Influence of filler geometry on melt strength of poly (lactid acid) composites with different electrically conductive fillers. Key Eng. Mater. 2014;605:449–452. doi: 10.4028/www.scientific.net/KEM.605.449. [DOI] [Google Scholar]
  74. Zhang X., Li L., Ouyang J., Zhang L., Xue J., Zhang H., Tao W.. Electroactive electrospun nanofibers for tissue engineering. Nano Today. 2021;39:101196. doi: 10.1016/j.nantod.2021.101196. [DOI] [Google Scholar]
  75. Ljungberg N., Wesslen B.. The effects of plasticizers on the dynamic mechanical and thermal properties of poly (lactic acid) J. Appl. Polym. Sci. 2002;86(5):1227–1234. doi: 10.1002/app.11077. [DOI] [Google Scholar]
  76. Van Nguyen S., Lee B.-K.. Polyvinyl alcohol/cellulose nanocrystals/alkyl ketene dimer nanocomposite as a novel biodegradable food packing material. Int. J. Biol. Macromol. 2022;207:31–39. doi: 10.1016/j.ijbiomac.2022.02.184. [DOI] [PubMed] [Google Scholar]
  77. Nguyen S. V., Lee B.-K.. Polyvinyl alcohol/alkyl ketene dimer films with excellent water resistance and water vapor barrier properties. Mater. Lett. 2022;307:131045. doi: 10.1016/j.matlet.2021.131045. [DOI] [Google Scholar]
  78. Zhang H.. Effect of a novel coupling agent, alkyl ketene dimer, on the mechanical properties of wood–plastic composites. Mater. Des. 2014;59:130–134. doi: 10.1016/j.matdes.2014.02.048. [DOI] [Google Scholar]
  79. Guo J., Tsou C.-H., Yu Y., Wu C.-S., Zhang X., Chen Z., Yang T., Ge F., Liu P., Guzman M. R. D.. Conductivity and mechanical properties of carbon black-reinforced poly­(lactic acid) (PLA/CB) composites. Iran. Polym. J. 2021;30(12):1251–1262. doi: 10.1007/s13726-021-00973-2. [DOI] [Google Scholar]
  80. Laraba S. R., Ullah N., Bouamer A., Ullah A., Aziz T., Luo W., Djerir W., Zahra Q. U. A., Rezzoug A., Wei J., Li Y.. Enhancing Structural and Thermal Properties of Poly­(lactic acid) Using Graphene Oxide Filler and Anionic Surfactant Treatment. Molecules. 2023;28(18):6442. doi: 10.3390/molecules28186442. [DOI] [PMC free article] [PubMed] [Google Scholar]
  81. Yuan Z., Wen Y.. Enhancement of hydrophobicity of nanofibrillated cellulose through grafting of alkyl ketene dimer. Cellulose. 2018;25(12):6863–6871. doi: 10.1007/s10570-018-2048-0. [DOI] [Google Scholar]
  82. Thananukul K., Kaewsaneha C., Roeurn B., Opaprakasit M., Kyaw Z. W., Khimlek W., Opaprakasit P.. Bifunctional Water-Based Alkyl Ketene Dimer Nanoparticles for Fabricating Cotton Fabrics with Hydrophobicity and Antimicrobial Properties. ACS Appl. Nano Mater. 2025;8(14):7224–7234. doi: 10.1021/acsanm.5c00586. [DOI] [Google Scholar]
  83. Song P., Cao Z., Cai Y., Zhao L., Fang Z., Fu S.. Fabrication of exfoliated graphene-based polypropylene nanocomposites with enhanced mechanical and thermal properties. Polymer. 2011;52(18):4001–4010. doi: 10.1016/j.polymer.2011.06.045. [DOI] [Google Scholar]
  84. Maciel M. M., Ribeiro S., Ribeiro C., Francesko A., Maceiras A., Vilas J. L., Lanceros-Méndez S.. Relation between fiber orientation and mechanical properties of nano-engineered poly­(vinylidene fluoride) electrospun composite fiber mats. Composites, Part B. 2018;139:146–154. doi: 10.1016/j.compositesb.2017.11.065. [DOI] [Google Scholar]
  85. Doungkom P., Jiamjiroch K.. Analysis of Printing Pattern and Infiltration Percent over the Tensile Properties of PLA Printed Parts by a Fuse Deposition Modelling Printer. IOP Conf. Ser.: Mater. Sci. Eng. 2019;501(1):012028. doi: 10.1088/1757-899X/501/1/012028. [DOI] [Google Scholar]

Articles from ACS Omega are provided here courtesy of American Chemical Society