Staged photothermal hydrogel containing manganese-doped bioactive glass nanoparticles promotes infected bone regeneration by engaging Schwann cell PI3K/AKT signaling and neuro-osteogenic coupling

Xinkai Cui a,1, Junxian Ma b,1, Zhenyu Yang a,1, Huiwen Luo a,1, Shiqi Dai a, Kai Tang a, Wen Niu a,⁎, Jihua Chen a,⁎⁎, Lina Niu a,⁎⁎⁎
PMCID: PMC13763574  PMID: 43032824

Abstract

Infected bone lesions are characterized by concurrent bacterial infection, persistent inflammatory infiltration, peripheral nerve damage, and impaired osteogenesis. However, most biomaterials address only antibacterial, anti-inflammatory, or osteogenic functions while overlooking nerve-bone crosstalk during tissue repair. Here, we engineered QOMB, an injectable photothermal hydrogel responsive to near-infrared (NIR) irradiation, by embedding manganese-doped bioactive glass nanoparticles (Mn-BGN) within a dynamically crosslinked network of gallic acid-grafted quaternized chitosan (QCSG) and oxidized sodium alginate (OSA). QOMB exerts synergistic photothermal antibacterial effects and promotes anti-inflammatory M2 macrophage polarization within inflammatory microenvironments. More importantly, ions released from Mn-BGN stimulate Schwann cells (SCs) to secrete abundant neurotrophic factors, thereby establishing a pro-regenerative paracrine niche that promotes osteogenic differentiation. Transcriptomic profiling and molecular validation demonstrated that stimulation with Mn-BGN-derived ionic cues activates PI3K/AKT signaling and enhances neurotrophic factor secretion by SCs. In a rat model of infected femoral condylar defects, QOMB administration combined with sequential NIR irradiation markedly suppressed local bacterial colonization, attenuated chronic inflammation, enhanced neurotrophic signaling, and accelerated de novo bone formation. These results support a material-Schwann cell-bone regulatory pathway that coordinates staged infection control and immune reprogramming with neuro-osteogenic repair.

Keywords: Infected bone defect repair, Neuro-osteogenic coupling, Temporal regulation, Bioactive glass nanoparticles, Photothermal hydrogel

Graphical abstract

graphic file with name ga1.webp

Highlights

  • •

    Mn-BGN-loaded Photothermal hydrogel QOMB was developed for infected bone repair.

  • •

    QOMB activates PI3K/AKT-dependent neurotrophic secretion in Schwann cells.

  • •

    Schwann cells act as a biological relay between ionic cues and osteogenic responses.

  • •

    QOMB combines antibacterial activity with macrophage-directed immunomodulation.

  • •

    Sequential PTT enables early antibacterial therapy and later regenerative support.

1. Introduction

Large bone defects caused by trauma, tumor removal, or surgical debridement remain difficult to reconstruct [1]. This problem becomes even more severe in the case of bone defects when infection is involved. With regard to bone defects involving infections, bacteria form biofilms and maintain inflammatory reactions that hinder bone tissue regeneration [2], [3]. The present-day approaches, which usually involve a combination of surgical debridement and antimicrobial treatment, are limited due to the lack of sufficient drug retention at the site of action, poor concentration control of antibiotics, development of antibiotic resistance, poor osteogenesis stimulation, and the presence of inflammatory microenvironment [4], [5]. A local material for this indication must therefore control infection and simultaneously restore conditions permissive for skeletal repair.

Recent designs have combined antimicrobial agents, immunoregulatory components, and osteogenic cues within a single scaffold or hydrogel [4], [6]. Through the combined action of eliminating the infection and regulating the local immunity, the systems create the optimal environment for the formation of bone tissue. However, the existing strategies are mostly concentrated on the regulation of local immunity and direct induction of osteogenesis, while the contribution of peripheral nerve injury and repair to bone regeneration remains largely overlooked. Peripheral neural elements are integral components of the skeletal microenvironment and actively participate in bone homeostasis and repair [7], [8], [9], [10], [11]. Neural ingrowth occurs during the early phase of skeletal healing and contributes to the regulation of bone formation and vascular responses [12], [13], [14]. Following tissue damage, Schwann cells (SCs), the major glial cells of the peripheral nervous system, adopt a repair-associated phenotype [15], [16], [17], [18], [19]. In addition to supporting axonal regeneration, activated SCs release nerve growth factor (NGF), glial cell line-derived neurotrophic factor (GDNF), and brain-derived neurotrophic factor (BDNF), whose effects can extend to osteogenic, vascular, and immune processes in injured tissue [10], [20], [21], [22], [23], [24], [25], [26], [27]. Thus, biomaterials that not only remove the pathogens from the area of injury but also resolve inflammation and activate Schwann cell-based neuro-osteogenic signaling are needed for complete repair of defects.

Manganese ions possess multifunctional bioactivities suitable for infectious bone therapy. Specifically, doping Mn into inorganic nanoparticles endows composites with adjustable photothermal conversion under NIR irradiation [28], [29]. Photothermal therapy (PTT) at controlled temperatures would be appropriate for staged bone defect repair. Short-duration heating at 45–50 °C can enhance bacterial killing through thermal damage to bacterial membranes and proteins, whereas prolonged exposure at this temperature may increase the risk of host-tissue injury. In contrast, mild hyperthermia at 40–42 °C provides a more cytocompatible thermal stimulus that can support osteogenic activity and bone regeneration [30], [31], [32], [33], [34], [35], [36], [37]. In addition, Mn2+ is widely recognized as an osteoactive ion [38], [39]. It supports matrix-associated enzymatic activity and may help increase cell adhesion and spreading through the action of integrins [40], [41]. Notably, manganese-based materials may partially enhance Schwann cell migration, facilitate axonal extension, and modulate the oxidative stress microenvironment [42], [43]. However, the neuroregulatory effects of Mn2+ are highly dose dependent, and excessive or prolonged exposure may induce neurotoxicity [44]. Precise control of Mn2+ concentration and release kinetics is therefore essential to harness its regenerative potential while minimizing adverse effects.

Bioactive glass nanoparticles (BGNs) are considered to be a reliable tool for delivering Ca, Si, and doped metal ions because of the degradation of the glass matrix and exchange reactions, which help to minimize the changes in the ion concentration locally [45]. Ca- and Si-containing dissolution products support apatite formation and osteogenic differentiation and can also shift macrophage responses toward a reparative state [46]. Beyond bone repair, bioactive glasses have also shown potential for peripheral nerve regeneration. Through ion release, surface bioactivity, and structural support, these materials can create a pro-regenerative microenvironment for neural cells, promote Schwann cell migration, and enhance Schwann cell-mediated neurotrophic paracrine signaling [47], [48]. Nevertheless, the direct application of BGNs to infected bone defects is limited by a mismatch between their degradation behavior in inflammatory microenvironments and the prolonged time course required for bone regeneration, as well as by their insufficient antibacterial activity [45]. An antibacterial carrier that retains BGNs locally and prolongs their therapeutic effects is therefore needed.

Hydrogels are well suited as local delivery platforms for BGN because of their extracellular matrix-like three-dimensional networks and excellent biocompatibility. However, conventional hydrogels often exhibit limited bioactivity and rapid degradation [49]. Gallic acid is a naturally occurring polyphenol with antibacterial, antioxidant, and anti-inflammatory activities. Incorporating gallic acid into hydrogel networks can increase network density and slow degradation [50], [51]. The resulting aromatic polyphenol network can also enhance light absorption and nonradiative energy dissipation [52]. These properties enable gallic acid to complement manganese-based nanomaterials and improve the photothermal conversion efficiency of the delivery system. These features make a gallic acid-functionalized hydrogel a suitable vehicle for BGN delivery.

We therefore incorporated Mn-BGN into a QCSG/OSA dynamic network to construct QOMB. Dynamic crosslinking through Schiff base reactions conferred injectability, self-healing capacity, and pH responsiveness. QOMB was designed to combine multiple bioactive functions, including immunomodulation by Mn, Si, and Ca ions and antibacterial activity conferred by gallic acid and quaternary ammonium groups. The combination of manganese and gallic acid also enabled efficient photothermal conversion, allowing temporally programmed PTT for antibacterial treatment during the early stage of injury and osteogenic stimulation during the subsequent regenerative phase. Importantly, we demonstrated that Mn-BGN incorporated into QOMB activated PI3K/AKT signaling in SCs, thereby enhancing their neurotrophic paracrine activity and ultimately promoting bone regeneration. By integrating antibacterial activity, anti-inflammatory regulation, and activation of SCs neurotrophic secretion, QOMB offers a multifunctional strategy for infected bone defect repair (Scheme 1).

Scheme 1.

Scheme 1

Schematic illustration of the fabrication of the QOMB hydrogel and its temporally coordinated treatment of infected bone defects. Mn-BGN, QCSG, and OSA were synthesized and assembled into the QOMB hydrogel through dynamic Schiff base crosslinking. Following implantation, high-temperature PTT was first applied for rapid bacterial control. During the subsequent phase, NIR treatment under mild-heating conditions and Mn2+, Ca2+, and SiO44− released by Mn-BGN promoted macrophage polarization toward a reparative phenotype and activated PI3K-AKT signaling in Schwann cells. The resulting enhancement of neurotrophic factor secretion established a Schwann cell-mediated neurotrophic paracrine microenvironment that supported neural repair and osteogenic regeneration.

2. Materials and methods

2.1. Materials

Ethanol (99%), dodecylamine (DDA), tetraethyl orthosilicate (TEOS), triethyl phosphate (TEP), sodium 2-(N-morpholino)ethanesulfonate (MES), Ca(NO3)2⋅4H2O (AR, 99%), and Mn(NO3)2·4H2O (AR, 99%) were acquired from Macklin (Shanghai, China). Ethylene glycol, acetic acid, glycidyltrimethylammonium chloride (GTMAC), gallic acid (GA), sodium periodate (NaIO4), sodium alginate (SA), 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC), and N-hydroxysuccinimide (NHS) were obtained from Aladdin (Shanghai, China). PBS, fetal bovine serum (FBS), α-MEM, and DMEM were supplied by Procell (Wuhan, China). Low-viscosity chitosan with a molecular weight of 1526.5 g/mol and a degree of deacetylation of 97.4% was used for QCS synthesis.

2.2. Synthesis and characterization of Mn-BGN

Mn-BGN with a nominal composition of 60SiO2-4P2O5-31CaO-5MnO (mol%) were prepared by a sol-gel route. DDA (1 g) was dissolved in 20 mL ethanol and 6.25 mL deionized water at 45 °C. After 20 min of stirring, TEOS (0.5 mL) was added in two portions separated by 10 min. TEP (51 μL) was added 30 min later, followed after 10 min by Ca(NO3)2·4H2O (274 mg in 0.5 mL deionized water) and, after a further 10 min, Mn(NO3)2·4H2O (48 mg in 0.5 mL deionized water). The reaction continued for 3 h. Particles were collected by centrifugation (10,000 rpm, 15 min), washed three times with ethanol and three times with deionized water, and lyophilized. Calcination was performed by heating at 2 °C/min to 350 °C for 3 h and then at 1 °C/min to 650 °C for 3 h, followed by furnace cooling. Particle morphology was examined by SEM and TEM. DLS/TEM size distributions and EDS elemental composition were quantified. XRD, XPS, and FTIR were used to characterize the amorphous structure and Mn chemical state.

2.3. Synthesis and characterization of QCSG and OSA

A previously published approach was slightly adjusted to synthesize QCS [50]. Low-viscosity chitosan (3 g) was dispersed in 120 mL of deionized water containing 600 μL of glacial acetic acid and maintained at 80 °C for 30 min. GTMAC (5 mL) was then added dropwise, and the reaction continued for 4 h. The product was precipitated with an acetone/ethanol mixture (1:1, v/v), collected, and dried under vacuum.

A procedure that has been reported before, with some slight adjustments, was used to manufacture QCS-g-gallic acid (QCSG) [51]. Gallic acid (170 mg) was dissolved in 100 mL of MES buffer (0.1 M, pH 6.0) and activated with EDC (20 mg) and NHS (55 mg) for 30 min at room temperature. After the pH was adjusted to 7.3, QCS (2 g) was introduced and the reaction mixture was stirred for 24 h. To get QCSG, the product was dialyzed and then lyophilized.

In order to synthesize OSA, 100 mL of deionized water was used to dissolve 1 g of SA. A solution of NaIO4 (210 mg in 5 mL of deionized water) was added dropwise, and oxidation proceeded for 2.5 h in the dark to limit periodate photodecomposition and uncontrolled side reactions. To remove any remaining NaIO4, 1 mL of ethylene glycol was added. The product was dialyzed against deionized water for 7 days, with the external water replaced every 8 h, and then lyophilized. Chemical changes in QCSG and OSA were assessed by FTIR spectroscopy (Thermo Scientific Nicolet iS20, USA).

The degree of quaternization of QCS was determined by 1H NMR spectroscopy based on the relative integral areas of the characteristic proton signals of the quaternary ammonium groups and the QCS backbone. The oxidation degree of OSA was determined by hydroxylamine hydrochloride titration. Briefly, 100 mg of OSA was reacted with hydroxylamine hydrochloride, and the released HCl was titrated with 0.1 M NaOH. The oxidation degree was calculated from the NaOH consumption according to the amount of aldehyde groups generated during alginate oxidation. The grafting degree of gallic acid onto QCS was quantified by UV–Vis spectroscopy. A series of gallic acid solutions with known concentrations were measured at 265 nm to establish a calibration curve. The absorbance of QCSG solution (0.5 mg/mL) was measured at the same wavelength, and the corresponding GA content was calculated from the calibration curve. The GA grafting degree was further calculated on a molar basis relative to the QCS repeating units.

2.4. Synthesis and characterization of QO and QOMB hydrogels

2.4.1. Synthesis of QO and QOMB hydrogels

The prepared QCSG and OSA were dissolved separately in PBS to obtain 5% (w/v) and 2% (w/v) solutions, respectively. Mn-BGN were ultrasonically dispersed in the QCSG solution to a final concentration of 5 mg/mL. OSA was then mixed with either QCSG solution alone or Mn-BGN-containing QCSG dispersion by magnetic stirring. Aldehyde-amine reactions produced gelation within 1 min. The Mn-BGN-containing hydrogel and the corresponding Mn-BGN-free hydrogel were designated QOMB and QO, respectively. In these abbreviations, Q, O, and MB represent QCSG, OSA, and Mn-BGN, respectively.

2.4.2. Microstructural characterization of the hydrogels

The microstructures of the QO and QOMB hydrogels were examined by SEM (ZEISS Sigma 360, Germany). Images were acquired at different magnifications to assess the porous architecture of the hydrogels. Pore-size distributions were quantified from the SEM images using ImageJ software, with at least five pores analyzed per group. Mn-BGN morphology during degradation was additionally examined by TEM after 5, 10, 15, and 30 days at pH 5 and 7. Zeta potential measurements were used to assess the electrostatic compatibility of positively charged QCSG and negatively charged Mn-BGN. Hydrogel porosity was determined using the ethanol displacement method. Each dry specimen was first weighed (W0), immersed in ethanol to saturation, blotted to remove surface liquid, and weighed again (W1). Porosity was calculated using the following equation:

Porosity = (W1 − W0) / (ρV) × 100%

where ρ denotes the density of ethanol and V is the apparent volume of the hydrogel specimen.

2.4.3. Photothermal performance and antioxidant activity of the hydrogels

QOMB formulations containing different Mn-BGN amounts were exposed to NIR laser (1.0 W cm−2) for 10 min. Surface temperature was measured continuously with an infrared thermal camera. Repeated heating–cooling cycles (6 min of irradiation and 4 min of natural cooling) were conducted to assess photothermal stability, during which the temperature was continuously monitored.

Antioxidant capacity was evaluated by DPPH radical scavenging. After incubation of the material extracts with DPPH, absorbance was recorded at 525 nm after background subtraction. Oxidative-stress protection was evaluated separately in MC3T3-E1 and RSC96 cells. Cells were challenged with 200 μM H2O2 for 24 h in the presence or absence of QO or QOMB extracts, and cell metabolic activity was subsequently quantified using the CCK-8 assay at 450 nm.

2.4.4. Mechanical property testing

Freshly combined QCSG and OSA precursor solutions were transferred immediately to the rheometer. Gel formation was followed by oscillatory time sweeps at an angular frequency of 10 rad/s and 1% strain, with storage modulus (G′) and loss modulus (G″) monitored continuously. Network recovery was evaluated by an alternating step-strain protocol at 1 Hz. QO and QOMB hydrogels were subjected to four repeated cycles of high strain (800%) and low strain (1%). The low-strain condition represented the intact hydrogel network, whereas the high-strain condition was applied to disrupt the network structure. Each strain interval was maintained for 120 s, and changes in G′ and G″ were monitored continuously throughout the test. Additional oscillatory tests compared hydrogels containing BGNs with 0, 5, and 10 mol% Mn substitution at the same particle loading. Flow measurements were recorded over 0.1-100 s−1 to characterize shear-thinning behavior.

2.4.5. Release of mn, Si, and Ca ions

To characterize pH-dependent ion release from the hydrogels, QO and QOMB hydrogels were separately immersed in 10 mL of Tris-HCl buffer or acetate buffer. At each sampling time, the entire medium was collected and replaced with an equal volume of fresh buffer of the same type. Mn, Si, and Ca concentrations were measured by ICP-OES (Agilent 5800, USA). The internal pH of hydrogels was measured by inserting a needle-type pH microelectrode into the center of the hydrogel at predetermined time points.

2.4.6. Swelling ratio and remaining mass

The swelling ratio and remaining mass of the hydrogels were determined by measuring the initial mass of the freeze-dried hydrogels (M0), their wet mass after immersion in PBS for different durations (M2), and their corresponding dried mass after immersion (M1). Three independent specimens were examined at each time point. Swelling and residual mass were calculated as follows:

Swelling ratio = (M2 – M0) / M0 × 100% (1)
Remaining mass = M1 / M0 × 100% (2)

2.5. Antibacterial properties

Antibacterial activity was determined against Staphylococcus aureus (S. aureus, ATCC 25923) and Escherichia coli (E. coli, ATCC 25922) under five conditions: (1) control, (2) QO, (3) QO + NIR, (4) QOMB, and (5) QOMB + NIR. The bacteria were obtained from the China General Microbiological Culture Collection Center (CGMCC, Beijing, China) and cultured in Luria–Bertani (LB) medium at 37 °C. For brevity in the figures and throughout the manuscript, QO + NIR and QOMB + NIR are denoted as QO+ and QOMB+, respectively. Bacterial suspensions were adjusted to 1 × 106 CFU/mL and incubated separately with the assigned hydrogel. The irradiated groups 3 and 5 received NIR laser exposure for 10 min. All co-culture systems were maintained for 8 h. Then the co-culture suspensions were collected for colony enumeration, bacterial live/dead staining, and morphological examination.

For CFU quantification, bacterial colonies were enumerated after serial dilution and spread plating of the co-culture suspensions. For live/dead staining, the suspensions were centrifuged to collect the bacteria. After a thorough washing with sterile saline, the bacterial pellets were dyed for 15 min in the dark using a bacterial viability/toxicity test. Afterwards, CLSM was used to analyze the labeled microorganisms. Bacteria taken from the co-culture suspensions were fixed in 2.5% glutaraldehyde, dehydrated through graded ethanol, and observed by SEM to assess cell-envelope morphology. To address established bacterial communities, preformed S. aureus and E. coli biofilms were also treated under the same material groups and evaluated by 3D live/dead confocal imaging and crystal-violet biomass quantification at 590 nm.

2.6. Cellular analyses

2.6.1. Cell culture

Murine preosteoblasts (MC3T3-E1), murine macrophages (RAW 264.7), and rat SCs (RSC96) were utilized. While MC3T3-E1 cells were maintained in α-MEM, RSC96 and RAW 264.7 cells were cultured in high-glucose DMEM. Cells from RAW 264.7 were gently detached by pipetting or scraping to minimize phenotypic changes, while cells from RSC96 and MC3T3-E1 were passaged with 0.25% trypsin-EDTA (Procell, China) at 80-90% confluence. Log-phase cells within appropriate passage ranges were used, and all cultures were routinely monitored for normal morphology and contamination. All cells were maintained at 37 °C in humidified 5% CO2. Culture media contained 10% FBS and 1% penicillin-streptomycin.

2.6.2. Biocompatibility of the hydrogels

Hydrogel extracts were fabricated by immersing QO and QOMB hydrogels in the corresponding culture medium (α-MEM or DMEM) for 24 h at 37 °C. The supernatants were collected, passed through a sterile 0.22-μm filter, and diluted to concentrations of 100%, 10%, 1%, and 0.1%. Cells cultured in hydrogel extract-free complete medium were employed as the negative control. We used RSC96 and MC3T3-E1 cells to test the biocompatibility of hydrogels. Cellular metabolic activity was quantified with Cell Counting Kit-8 (CCK-8; Elabscience, China), and absorbance at 450 nm was recorded with a microplate reader. After 48 h, calcein-AM/PI staining (Elabscience, China) was used to visualize viable and dead cells by CLSM. QOMB was extracted in DMEM at a material-to-medium ratio of 100 mg/mL for 24 h at 37 °C. To define the ionic exposure used in the in vitro experiments, QOMB extracts were analyzed by ICP-OES.

2.6.3. In vitro neurogenic activity of the hydrogels

RSC96 cells were exposed to hydrogel extracts for 2 days, fixed, and immunostained using antibodies against BDNF (28205-1-AP; Proteintech, China), NGF (ab52918; Abcam, USA), and GDNF (GB11403; Servicebio, China). Clarified culture supernatants were analyzed for secreted BDNF and GDNF using ELISA kits (Elabscience, China; Boster, China). In parallel, total RNA and protein were collected from treated SCs for RT-qPCR and Western blotting, respectively. Component-control experiments additionally compared QO, QO + BGN, QO + Mn, and QOMB. In the QO + BGN group, QO was loaded with BGN without Mn doping. In the QO + Mn group, MnCl2 was added to QO to provide an Mn2+ concentration equivalent to that detected in the QOMB hydrogel extract. For pathway validation, RSC96 cells were analyzed under Control, LY294002, QOMB, QOMB + LY294002, and QOMB + LY294002+SC79 conditions. For brevity in the figures, LY294002, QOMB + LY294002, and QOMB + LY294002+SC79 are denoted as LY, QOMB + LY, and QOMB + LY + SC79, respectively. LY294002 and SC79 were each used at 20 μM for 24 h. p-PI3K/PI3K, p-AKT/AKT, p-CREB/CREB, BDNF, and NGF were quantified from three independent WB experiments.

2.6.4. Hydrogel-stimulated neuro-osteogenic coupling

The effects of RSC96-conditioned medium on osteogenic differentiation were examined by exposing RSC96 cells to QO or QOMB hydrogel extracts for 48 h. After removing the serum-containing medium, the RSC96-conditioned medium was collected 24 h later. MC3T3-E1 cells received a 1:1 (v/v) mixture of osteogenic induction medium and conditioned medium for 48 h before replacement with fresh medium. For the in vitro NIR treatment (808 nm, 5 W cm−2), the medium temperature was monitored, with an initial heating period followed by 10 min of maintenance at 40-42 °C. To test the contribution of Schwann-cell neurotrophic signaling, QOMB-conditioned medium was separately subjected to BDNF-, GDNF-, or NGF-neutralizing antibody treatment before application to MC3T3-E1 cells. In a separate pathway-relay experiment, conditioned media were collected from RSC96 cells subjected to Control, LY294002, QOMB, QOMB + LY294002, or QOMB + LY294002+SC79 treatment and subsequently applied to MC3T3-E1 cells. To distinguish the direct osteogenic effects of hydrogel-derived components from Schwann cell-mediated paracrine effects, MC3T3-E1 cells were cultured with QO or QOMB extracts, with or without NIR irradiation. Alkaline phosphatase (ALP) staining and Alizarin Red S (ARS) staining were conducted on days 7 and 14, respectively, to assess early bone differentiation and extracellular matrix mineralization. Immunofluorescence (IF) staining was performed using antibodies against Col1A1 (AF7001; Affinity, China), Ocn (DF12303; Affinity, China), and Runx2 (AF5186; Affinity, China). Total RNA and protein were also collected for RT-qPCR and WB, respectively (n = 3).

2.6.5. Macrophage polarization analysis

RAW 264.7 cells were stimulated with 1 μg/mL lipopolysaccharide (LPS) for 12 h to induce the pro-inflammatory phenotype and subsequently exposed to hydrogel extracts for 48 h. These cells were collected for flow cytometry and IF staining using antibodies against CD86 (DF6332; Affinity, China) and CD206 (DF4149; Affinity, China). Total RNA and protein were collected for RT-qPCR and WB to assess macrophage polarization. All quantitative experiments were performed with three independent biological replicates (n = 3).

2.6.6. RT-qPCR and WB

Total RNA was isolated from RAW264.7, MC3T3-E1, and RSC96 cells with TRIzol reagent (Servicebio, China). Complementary DNA (cDNA) was synthesized using the PrimeScript FAST RT Reagent Kit with gDNA Eraser (Takara, Japan). RT-qPCR was carried out in 20-μL TB Green Premix Ex TaqII reactions (Takara, Japan) on a real-time PCR system. Relative transcript abundance was normalized to GAPDH and calculated by the 2−ΔΔCt method. Primer sequences are provided in Table S1.

Proteins were extracted in radioimmunoprecipitation assay (RIPA) lysis buffer (Elabscience, China), and concentrations were quantified by bicinchoninic acid (BCA) assay (Epizyme, China). Equivalent protein amounts were resolved by SDS–PAGE and transferred to 0.45-μm polyvinylidene difluoride (PVDF) membranes (Millipore, USA). After blocking with 5% nonfat milk for 1 h, membranes were incubated overnight at 4 °C with antibodies against iNOS (AF0199; Affinity, China), CD86 (DF6332; Affinity, China), CD206 (DF4149; Affinity, China), Arg-1 (DF6657; Affinity, China), ALP (AF2910; R&D Systems, USA), Col1A1 (A1352; Abclonal, China), Ocn (DF12303; Affinity, China), Runx2 (AF5186; Affinity, China), AKT (10176-2-AP; Proteintech, China), phospho-AKT (p-AKT; 66444-1-Ig; Proteintech, China), BDNF (28205-1-AP; Proteintech, China), NGF (ab52918; Abcam, USA), PI3K (AF6242; Affinity, China), phospho-PI3K (p-PI3K; AF3242; Affinity, China), CREB (9197; CST, USA), and phospho-CREB (p-CREB; 9198; CST, USA). Enhanced chemiluminescence reagent was used to observe protein bands after incubating the membranes with horseradish peroxidase-conjugated secondary antibodies following washing.

2.6.7. RNA sequencing and data analysis

RSC96 samples were collected under Control, QO, and QOMB conditions after 48 h, allowing QOMB-vs-QO, QOMB-vs-Control, and QO-vs-Control comparisons. MC3T3-E1 transcriptomic analysis compared cells exposed to QO- and QOMB-derived Schwann-cell-conditioned media after 7 days. RNA quality control, library preparation, sequencing, and primary processing were performed by OmicsMaster (China). Genes with |log2(fold change)| > 1 and adjusted P < 0.05 were defined as DEGs. GO, KEGG, and GSEA were used for functional interpretation.

2.7. In vivo experiments

All animal procedures were approved by the Experimental Animal Welfare and Ethics Committee of the Hospital of Stomatology, Fourth Military Medical University (permission no. IACUC-2025-kq-071). We used male Sprague-Dawley rats that were around six or seven weeks old. A sterile drill was used to generate a cylindrical defect in the femoral condyle, with dimensions of 3 mm in diameter and depth. After hemostasis, 20 μL of a Staphylococcus aureus suspension (1 × 108 CFU/mL) was injected into the defect. One week after infection, the rats were randomly allocated to control, QO, QOMB, QO+, and QOMB + groups and excluded from analysis only if predefined criteria were met, including failure to establish the infected bone-defect model, unexpected perioperative death unrelated to the experimental treatment, or technical damage to specimens that precluded reliable analysis. No animals met these criteria or were excluded from the final analysis. Before initiating the animal experiments, an a priori power analysis was performed to determine the required sample size based on the prespecified primary comparison of BV/TV at 8 weeks between the QOMB+ and QO + groups. Based on previously published bone regeneration studies [53], [54], [55], an anticipated between-group difference of 15 percentage points and a common within-group standard deviation (SD) of 4 percentage points were assumed. For the balanced five-group design, the analysis incorporated Tukey's multiple-comparison adjustment, with a family-wise significance level of α = 0.05 and a target statistical power of 80%. The estimated power was 49.45% for n = 2 and 86.80% for n = 3 animals per group. Accordingly, three animals per group were selected as the minimum sample size meeting the predefined power requirement. The control group underwent debridement without hydrogel implantation. In the QO and QOMB groups, the infected defects were debrided and filled with the corresponding hydrogel using a syringe. The QO+ and QOMB + groups received the corresponding hydrogels after debridement, followed by NIR irradiation according to the photothermal treatment protocol. In the irradiated groups, an 808 nm laser was initially applied at 1.0 W cm−2 until the defect-surface temperature reached the prescribed target range. The power density was subsequently fixed at 0.8 W cm−2 during the antibacterial phase and 0.6 W cm−2 during the osteogenic phase to maintain the respective target temperature ranges for an additional 10 min, with real-time infrared thermographic monitoring. On days 1-3, treatment was given once daily while the defect-surface temperature was maintained at 45-50 °C. Six additional sessions were performed on days 4, 6, 8, 10, 12, and 14 at 40-42 °C, giving a total of nine sessions and 90 min of target-temperature maintenance, excluding the initial heating periods. The representative initial heating periods were approximately 6 min and 3 min for the antibacterial and mild-heating phases, respectively. The single-session thermal exposure was estimated from the representative defect-surface temperature profiles as cumulative equivalent minutes at 43 °C (CEM43), incorporating both the initial heating and target-temperature maintenance periods. To evaluate potential early thermal injury, bone defect tissues were collected on day 3 from the Control, NIR, QOMB, and QOMB + groups for H&E and TUNEL staining. The NIR group received 808 nm irradiation without hydrogel implantation, using the same power densities and irradiation durations. Early defect tissue was additionally collected for quantitative bacterial colony counting.

Femoral condyles were harvested at 4 and 8 weeks for micro-CT, H&E, Masson staining, and immunostaining. Schwann-cell-associated apoptosis was evaluated by S100β/TUNEL co-staining. Total Mn in defect-associated bone and blood was measured by ICP-OES at the indicated early time points, and H&E sections of heart, liver, spleen, lung, and kidney were examined for systemic histopathology. Runx2, Ocn, and Bmp2 were used to assess osteogenic activity. S100β/BDNF and S100β/NGF co-immunofluorescence, together with NF200 staining, was used to evaluate Schwann-cell-associated neurotrophic signals and neural ingrowth and thresholded Manders M2 (tM2) was used for colocalization quantification. CD68/CD86 and CD68/CD206 co-staining was used to assign inflammatory markers to macrophages.

2.8. Statistical analysis

ImageJ was used to quantify the experimental images. Statistical calculations were performed in SPSS, and graphical representations were prepared with GraphPad Prism. All quantitative results are expressed as the mean ± standard deviation (SD). Two-group comparisons used a two-tailed Student's t-test, whereas datasets containing more than two groups were analyzed by one-way analysis of variance (ANOVA) followed by Tukey's post hoc test. P < 0.05 was considered statistically significant.

For in vivo outcomes, the individual rat was the unit of analysis, and 4- and 8-week data were analyzed separately. Multiple sections or microscopic fields were averaged within each animal before between-group testing. In addition to one-way ANOVA with Tukey post hoc comparisons, the overall effect size was summarized using omega-squared (ω2), and pairwise standardized effect sizes were estimated using Hedges’ g. Pairwise mean differences are reported with Tukey-adjusted 95% confidence intervals (CIs). Detailed analyses of all 12 in vivo endpoints at both time points are reported in Tables S2 and S3.

3. Results and discussion

3.1. Synthesis and characterization of Mn-BGN

Monodisperse spherical Mn-BGN particles were fabricated through the sol-gel procedure (Fig. 1a). TEM elemental mapping verified the uniform distribution of Mn throughout the glass matrix (Fig. 1b). Energy-dispersive X-ray spectroscopy (EDS) further demonstrated the expected elemental constituents of Mn-BGN (Fig. S1a). ICP-OES analysis revealed Si, Ca, Mn, and P contents of 24.27, 14.11, 3.95, and 3.37 wt%, respectively. The measured Mn content corresponded to 88.2% of the theoretical value calculated from the precursor composition (4.48 wt%). FTIR results of the nanoparticles revealed that the absorption bands at 3435 and 477 cm−1 were assigned to H-O-H and Mn-O bonds, respectively, whereas the peaks at 1068 and 796 cm−1 corresponded to the asymmetric and symmetric Si-O-Si stretching, respectively (Fig. S1b) [28], [29]. XPS was used to determine the oxidation state of Mn. The Mn 2p spectrum exhibited characteristic peaks corresponding to Mn2+ 2p1/2 and Mn2+ 2p3/2, supporting incorporation of divalent manganese into the particles (Fig. 1c), consistent with previous reports [29]. The SEM images also confirmed the presence of a uniform spherical shape of Mn-BGN (Fig. S1c). Moreover, the HRTEM images, XRD patterns, and SAED confirmed the absence of any crystal lattice planes, peaks, or rings. This all suggests that the Mn-BGN still retains its amorphous nature after the addition of Mn ions (Fig. S1d–f). Quantitative sizing gave a mean TEM diameter of approximately 260.6 nm, whereas DLS showed a larger hydrodynamic diameter (approximately 849.5 nm). The larger hydrodynamic diameter measured by DLS is attributable to the hydration layer and possible particle association in suspension (Fig. S2a and b).

Fig. 1.

Fig. 1

The preparation and characterization of Mn-BGN and QOMB hydrogel. (a) TEM image of Mn-BGN. Scale bar: 100 nm. (b) TEM elemental mapping images of Mn-BGN. Scale bar: 100 nm. (c) XPS of Mn−BGN, showing the valence states of the element manganese. (d) SEM images of QO and QOMB scaffold. (e) FTIR spectra of QCS, QCSG and OSA. (f) The temperature change curve of QOMB hydrogels containing different amounts of Mn-BGN under NIR irradiation. (g) Photothermal cycling behavior of QOMB hydrogels containing 0.5% Mn-BGN. (h) Time-sweep rheological profiles of QO and QOMB hydrogels. (i) Step-strain rheological analysis demonstrating the self-recovery of QO and QOMB hydrogels under alternating low and high strains. (j, k) Comparison of pore sizes and porosity of QO and QOMB hydrogels (n = 5). (l) Injectability of the hydrogel through a syringe. (m) Self-healing behavior of the hydrogel after cutting and rejoining. ICP-OES analysis of the (n) Si and (o) Mn released concentrations. (p) Swelling curves and (q) degradation curves of QO and QOMB hydrogels. Data are presented as means ± SD, **p < 0.01, ***p < 0.001.

3.2. Synthesis and characterization of QOMB hydrogels

In order to provide a sustained release of bioactive ions from Mn-BGN and increase the effectiveness of the system with respect to antibacterial, anti-inflammatory, and photothermal activity, Mn-BGN was first dispersed in QCSG and then combined with OSA. QOMB hydrogels were obtained through Schiff base condensation reaction and ionic interaction. SEM showed that QO and QOMB hydrogels had an interconnected porous structure, and that Mn-BGN was uniformly distributed in QOMB hydrogel (Fig. 1d). Both QCS and QCSG showed a distinct absorption band at approximately 1480 cm−1, which corresponded to the methyl groups of glycidyl trimethylammonium chloride (GTMAC), thereby confirming the successful quaternization of chitosan (Fig. 1e). The characteristic peaks observed at 880-680 and 1600-1450 cm−1 corresponded to the bending vibrations of aromatic C-H bonds and the stretching vibrations of benzene-ring C=C bonds, respectively. These spectral features indicated that gallic acid had been successfully conjugated to QCS, in agreement with previously published findings [50], [51]. In addition, the FTIR spectrum of OSA exhibited a weak band near 1726 cm−1, which was assigned to the carbonyl stretching vibration of aldehyde moieties. The appearance of this signal validated the successful oxidative modification of sodium alginate. Quantitative analysis further confirmed the chemical modification of the hydrogel precursors. The degree of quaternization of QCS determined by 1H NMR was 47.0% (Fig. S2c), while hydroxylamine hydrochloride titration gave an OSA oxidation degree of 18.6 ± 0.3%. UV–Vis spectra supported GA grafting onto QCS (Fig. S2f), with a grafting degree of approximately 7.1 mol% determined using the GA calibration curve. Notably, GA was covalently conjugated to the QCS backbone rather than physically incorporated as a freely diffusible molecule. This configuration is expected to restrict the rapid diffusion of free GA and mitigate the initial burst release associated with conventional physically loaded systems. Previous studies have highlighted the importance of polymer crosslinking and molecular interactions in regulating GA release kinetics [56]. QCSG showed a positive zeta potential (+33.3 mV), whereas Mn-BGN was negatively charged (−24.8 mV). Their electrostatic attraction may facilitate interfacial association and improve nanoparticle dispersion within the hydrogel network (Fig. S2d and e).

The photothermal properties of QOMB hydrogels with different amounts of Mn-BGN were investigated systematically (Fig. 1f and Fig. S5a). When exposed to 808 nm NIR irradiation, there is an obvious increase in the rate of temperature change depending on increasing Mn-BGN content. Such a result implies that Mn-BGN enhances the photothermal effect significantly and helps produce heat in the QO hydrogels. Compared to QO and QOMB with 1% of Mn-BGN, QOMB with 0.5% of Mn-BGN is capable of better controlling the temperature in the range of 40-42 °C, which is optimal for osteogenesis. Therefore, the concentration of 0.5% of Mn-BGN was chosen for the following tests. Additionally, the photothermal cycling tests revealed that QOMB can sustain its heating ability through five cycles of irradiation (Fig. 1g). The subsequent staged photothermal treatment was implemented through an externally prescribed NIR irradiation protocol, with QOMB providing the photothermal responsiveness required to achieve the selected temperature ranges rather than autonomously controlling the timing of each phase.

Rheological behavior of the hydrogels was investigated to confirm network establishment and dynamic recovery ability. Time sweep tests revealed that for both QO and QOMB, the storage moduli consistently exceeded the loss moduli throughout the test period. The findings prove the formation of stable gel networks with mainly elastic nature (Fig. 1h). Notably, the storage modulus value of QOMB was much higher compared to QO, thus suggesting the strengthening of the hydrogel network by Mn-BGN. Comparative rheology with 0, 5, and 10 mol% Mn-substituted BGNs showed that increasing Mn substitution increased G′ while G′ remained higher than G″, indicating reinforcement without loss of gel-like behavior (Fig. S2g). Healing of the hydrogels was evaluated by performing alternating step-strain rheological analysis. In the case of low strain values, the storage modulus was higher, which suggests that the hydrogel structure was maintained. Once subjected to high strains, the storage modulus decreased dramatically and became smaller than the loss modulus, implying that the network structure of the hydrogels was disrupted. After the strain was lowered, the storage modulus increased and once again became larger than the loss modulus for several cycles. This shows that healing of the hydrogel network occurs successfully after its mechanical destruction (Fig. 1i). This reversible transition was mainly attributed to dynamic Schiff base bonds and reversible noncovalent forces inside the hydrogel matrix. The incorporation of Mn-BGN shortened the gelation time of the QCSG/OSA network with increasing Mn-BGN concentration (Fig. S5b). Compared with QO, the porous architecture of QOMB had smaller pores and lower porosity (Fig. 1j and k). The improved porous structure can be attributed to the inclusion of Mn-BGN, as this can result in the strengthening of the polymer network by ionic coordination of Mn-BGN and OSA. The denser porous structure of QOMB was in agreement with the improved mechanical robustness of the hydrogel. The capacity for injection and self-healing was further confirmed. Fig. 1l shows the good injectability of the hydrogel, which can be used in the minimally invasive injection of the irregular bone defects. The viscosity decreased continuously over the tested shear-rate range (0.1-100 s−1), demonstrating shear-thinning behavior rather than a discrete injection threshold (Fig. S2h). In addition, the hydrogel, when divided into two pieces, instantly got joined and retained its structure without any external stimuli, proving the ability of self-healing of the hydrogel (Fig. 1m). These properties were attributed primarily to reversible dynamic interactions within the hydrogel network and were consistent with the rheological findings shown in Fig. 1i.

ICP-OES showed sustained Mn, Si, and Ca release from QOMB under both neutral and acidic conditions, with a markedly accelerated release profile under acidic conditions (Fig. 1n, o and Fig. S3b). TEM during degradation showed progressive disruption of the Mn-BGN particles, particularly at pH 5, consistent with the ion-release profiles (Fig. S3a). The acid-responsive nature of these materials is attributed to the Schiff-base linkages and could allow for the QOMB to better adapt to the acidic environment within infected defects and deliver bioactive ions locally during tissue healing. In addition, the swelling of both QO and QOMB was observed with subsequent degradation over a prolonged period of time (Fig. 1p and q), which suggests good fluid intake along with the persistence of structure. The intragel pH of QOMB remained approximately 7.0–7.4 under both neutral and acidic conditions. This pH stability was likely attributable to the buffering capacity of PBS, which constituted the aqueous phase of the hydrogel. QO and QOMB exhibited DPPH radical-scavenging activity, with a higher scavenging rate for QOMB. In H2O2-challenged MC3T3-E1 and RSC96 cells, both materials improved cell viability, and QOMB produced the greater recovery (Fig. S4). These results support antioxidant protection from the GA-containing network with an additional Mn-BGN-associated contribution.

3.3. Antibacterial properties of the hydrogels

The antibacterial properties of QO and QOMB were systematically assessed with and without photothermal treatment. Both hydrogels effectively inhibited bacterial growth. Colony-counting assays revealed pronounced antibacterial activity in the QO and QOMB groups, although small numbers of surviving S. aureus and E. coli colonies remained detectable (Fig. 2a–c). And the lowest colony numbers were observed in the QO+ and QOMB + groups, supporting a robust synergistic antibacterial effect between the hydrogels’ inherent antibacterial properties and PTT (Fig. 2a–c). Live/dead staining also revealed abundant viable bacteria in the control group but extensive bacterial death after co-culture with QO or QOMB. And PTT further enhanced the bactericidal effect (Fig. 2d). In addition, preformed-biofilm assays showed reduced biomass by crystal-violet staining and increased dead-bacteria signal in 3D confocal images, with the strongest effect in QOMB+ (Fig. S6).

Fig. 2.

Fig. 2

Antibacterial testing of the hydrogels. (a) Representative images of S. aureus and E. coli colonies with different treatments. Colony counting of (b) S. aureus and (c) E. coli with different treatments (n = 3). (d) Live/dead staining of S. aureus and E. coli colonies in different treatment groups. Scale bar: 100 μm. (e) Representative SEM images of S. aureus and E. coli colonies with different treatments. Scale bar: 1 μm. Data are presented as means ± SD, *p < 0.05, ****p < 0.0001.

To further investigate the antibacterial mechanism, bacterial morphology was examined by SEM (Fig. 2e). For the control group, the bacteria displayed smooth and undamaged surfaces with typical coccal or bacillary structures. On the other hand, the bacteria of all the groups treated with hydrogel exhibited significant surface shrinking, cell membrane destruction, and leakage of cytoplasmic content. Such structural changes were especially obvious in the case of QO+ and QOMB + groups, indicating that PTT additionally aggravates the damage of the bacterial membrane. Overall, the findings support enhanced bacterial membrane damage and bacterial elimination by the combined hydrogel-NIR treatment.

The inherent antibacterial properties of QCSG are attributed mainly to the effects produced by the QCS together with the grafted gallic acid functionalities. Compared to the natural chitosan, the quaternization process gives stable positive charges to the QCSG at physiological conditions, thus enhancing the ability of forming electrostatic interaction with the negatively charged bacterial envelopes [57]. The electrostatic interactions could lead to the disruption of membrane integrity, increased permeability, and the release of the cellular components of the bacteria, hence reducing the ability of the bacteria to thrive. In addition, the phenolic structure of the grafted gallic acid functionalities may enhance the antibacterial effects through the interactions with the bacterial membranes [58], [59]. This contact-killing mechanism provides an antibiotic-free strategy for reducing bacterial burden in infected bone defects and can be further enhanced by high-temperature PTT.

3.4. Immunomodulatory properties of the hydrogels

Excessive and persistent inflammation can impair bone tissue repair in infected bone defects [60], [61], [62]. Establishing a local immune microenvironment (IME) conducive to tissue regeneration is therefore essential. The effect of the hydrogels on the modulation of immune responses in inflammation was studied by exposing the cells to stimulation using LPS followed by addition of QO or QOMB with or without 808 nm NIR irradiation. IF staining demonstrated that LPS triggered a considerable upregulation of the M1 marker CD86 and a decrease in the M2 marker CD206 (Fig. 3a–c). Hydrogel treatment reversed these changes, as evidenced by decreased CD86 expression and increased CD206 expression. The anti-inflammatory activity of QO may be partly attributable to the gallic acid moieties within the hydrogel network. Notably, QOMB induced a more pronounced transition to the M2 phenotype than QO, possibly because of the Mn and Si released from Mn-BGN. Moreover, 808 nm NIR irradiation further enhanced the acquisition of an anti-inflammatory phenotype, suggesting that NIR treatment under mild-heating conditions modulated macrophage responses in conjunction with hydrogel-derived components.

Fig. 3.

Fig. 3

In vitro immunomodulation and macrophage activation by different hydrogels without/with NIR irradiation. (a) Fluorescence images of CD86 and CD206 (red: CD86, green: CD206, blue: DAPI). Scale bar: 50 μm. Relative fluorescence intensity of (b) CD86 and (c) CD206 staining (n = 3). (d) Western blot analysis of protein expression of CD86, iNOS, Arg-1, CD206, and β-tubulin after 2 days of culture. (e) Flow cytometry of the M1 and M2 macrophages in RAW 264.7 cells. RT-qPCR analysis of mRNA expression levels of (f) iNOS, (g) TNF-α, (h) CD206 and (i) Arg-1 after 2 days of different treatments of RAW 264.7 cells (n = 3). Data are presented as means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001.

Further validation was done using WB and flow cytometry experiments (Fig. 3d, e and Fig. S7). The macrophages, which were incubated with the hydrogel, showed enhanced CD206 and Arg-1 expressions while displaying reduced CD86 and iNOS expressions. Using RT-qPCR analysis, similar trends were observed with the increased expressions of CD206 and Arg1 along with reduced expressions of iNOS and TNF-α (Fig. 3f–i). In summary, QO, Mn-BGN integration, and NIR irradiation work in combination to convert macrophages to a reparative state from a pro-inflammatory one, thereby providing a favorable immunological microenvironment for neuro- and osteo-regeneration.

3.5. QOMB-mediated enhancement of neurotrophic factor secretion by SCs

The effects of the hydrogels on Schwann cell viability and trophic activity were evaluated using RSC96 cells. Because the cumulative release profile of the hydrogel does not directly represent the ionic dose experienced by cells during extract treatment, the 24-h QOMB-DMEM extract was analyzed by ICP-OES. The measured concentrations were 0.853 mg/L Mn, 13.72 mg/L Ca, and 10.67 mg/L Si. While no difference in cell viability was detected across all groups on day 1 by CCK-8 assay, the treated groups exhibited a notably enhanced RSC96 cell proliferation rate on days 3 and 5 post-seeding relative to the control (Fig. 4a). Similarly, live/dead staining performed after 48 h showed a similar cell viability between control and hydrogel extract treated cells, with the majority of cells being viable in all groups (Fig. 4b). These findings supported the favorable cytocompatibility of the hydrogels and suggested that the hydrogel-derived microenvironment promoted Schwann cell proliferation during prolonged culture. The favorable early cytocompatibility may be partly associated with the covalent immobilization of GA within the QCSG/OSA network, which is expected to limit rapid exposure to freely diffusible GA during the initial culture period.

Fig. 4.

Fig. 4

Enhancement of Schwann cell neurotrophic secretion by QOMB. (a) The survival rate of RSC96 was assessed at 1, 3, and 5 days using the CCK-8 assays. (b) Double staining of live/dead cells. Scale bar: 50 μm. (c) Fluorescence images of NGF (red: NGF, blue: DAPI) in RSC96 after 2 days of treatment. Scale bar: 100 μm. (d) Fluorescence images of BDNF (green: BDNF, blue: DAPI) in RSC96 after 2 days of treatment. Scale bar: 100 μm. (e) Fluorescence images of GDNF (green: GDNF, blue: DAPI) in RSC96 after 2 days of treatment. Scale bar: 100 μm. RT-qPCR analysis of gene expression for (f) BDNF, (g) GDNF, and (h) NGF (n = 3). ELISA quantification of (i) BDNF and (j) GDNF secretion by RSC96 cells after different treatments (n = 3). Data are presented as means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001.

We subsequently investigated the influence of hydrogels on the neurotrophic characteristics of RSC96 cells. IF staining revealed comparable expression of BDNF, GDNF, and NGF between the control and QO groups, which suggested that QO exerted little influence on the expression of neurotrophic factors secreted by SCs. However, the fluorescence intensities of GDNF, NGF, and BDNF were markedly increased in the QO+, QOMB, and QOMB + groups, with the strongest signals observed in the QOMB + group (Fig. 4c–e and Fig. S8a–c). RT-qPCR analysis after 2 days of culture showed a similar trend in GDNF, NGF, and BDNF mRNA expression (Fig. 4f–h). These findings indicate that Mn-BGN-associated soluble cues and NIR treatment under mild-heating conditions enhanced the neurotrophic response of Schwann cells. Additional component controls showed that both non-Mn BGN and soluble Mn produced partial increases in BDNF/GDNF/NGF-related readouts, whereas QOMB produced the strongest response (Fig. S9). These data argue against assigning the effect exclusively to Mn or BGN and instead support a combined Mn-BGN-associated ionic microenvironment involving Mn together with Si/Ca dissolution products.

To investigate whether this enhanced neurotrophic response was accompanied by increased factor secretion, BDNF and GDNF concentrations in RSC96 culture supernatants were quantified by ELISA. QOMB increased the secretion of both neurotrophic factors (Fig. 4i and j). Thus, QOMB not only promoted intracellular neurotrophic factor expression but also enhanced the neurotrophic secretory function of SCs. Given the important roles of neurotrophic factors in neuro-osteogenic coupling, these findings suggested that QOMB may establish a paracrine microenvironment that indirectly promotes bone regeneration.

3.6. Mechanistic Elucidation and validation of QOMB-induced neurotrophic activation in SCs

To investigate the mechanism by which QOMB promotes the Schwann-cell neurotrophic response, RNA sequencing was performed after 2 days. The QOMB-vs-QO comparison identified 486 DEGs, including 298 upregulated and 188 downregulated genes (Fig. 5a). The heatmap further showed a distinct transcriptional profile in QOMB-treated cells (Fig. 5b). GO enrichment linked these changes to extracellular-region activity, cell-substrate adhesion, neuron migration, metal-ion transport, exocytosis, calcium-ion transport, growth-factor activity, and neuron projection development (Fig. 5c). KEGG analysis showed enrichment of PI3K/AKT, MAPK, HIF-1, Ras, focal adhesion, integrin, and calcium signaling pathways (Fig. 5d). GSEA further demonstrated positive enrichment of the PI3K/AKT signaling pathway and regulation of glial cell differentiation in the QOMB group (Fig. 5e and f). We additionally analyzed QOMB-vs-Control and QO-vs-Control contrasts (Figs. S10 and S11). The added comparisons showed that the polymer network itself produced a measurable but more limited transcriptional response, whereas the QOMB profile contained the stronger neurotrophic and PI3K/AKT-associated signatures. These three contrasts are now considered together rather than treating QO as the only baseline.

Fig. 5.

Fig. 5

Transcriptomic analysis and mechanistic validation of QOMB-induced Schwann cell neurotrophic activation. (a) Volcano plot of the upregulated and downregulated genes in the QOMB group compared to the QO group. (b) Heatmap depicting the DEGs associated with the vesicular transport and neural repair of the QO group and the QOMB group. (c) GO enrichment analysis of upregulated DEGs. (d) KEGG enrichment analysis of upregulated DEGs. (e) GSEA of the PI3K/AKT signaling pathway. (f) GSEA of regulation of glial cell differentiation. (g) Western blot analysis of protein expression of PI3K, p-PI3K, AKT, p-AKT, CREB, p-CREB, BDNF, NGF, and β-tubulin. Quantitative analysis of (h) p-PI3K/PI3K and (i) BDNF expression. Data are presented as means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001.

PI3K/AKT was selected for pharmacological follow-up because it was consistently enriched in the transcriptomic analysis and is closely associated with Schwann-cell survival and neurotrophic regulation. The enrichment of MAPK and HIF-1 signaling also indicates that the QOMB-induced response is not restricted to PI3K/AKT. In addition, the enrichment of focal adhesion, integrin and calcium signaling is consistent with changes in cell-matrix interaction and intracellular signaling, while the positive enrichment of glial cell differentiation further supports a shift in Schwann-cell functional state.

Pharmacological inhibition-rescue experiments provided functional support for the PI3K/AKT-CREB branch. LY294002 reduced p-PI3K/PI3K, p-AKT/AKT, p-CREB/CREB, BDNF, and NGF relative to QOMB. Addition of the downstream AKT activator SC79 restored p-AKT and p-CREB and substantially rescued BDNF/NGF, while upstream p-PI3K remained suppressed (Fig. 5g-i and Fig. S12). This response pattern is consistent with pathway order and supports a functional PI3K-to-AKT-to-CREB contribution to the QOMB-induced neurotrophic phenotype.

3.7. Hydrogel-mediated neuro-osteogenic coupling

CCK-8 analysis revealed comparable cell viability across all groups (Fig. S13a). Live/dead imaging at 48 h likewise showed widespread cell survival (Fig. S13b), supporting the cytocompatibility of the tested hydrogel extracts. To evaluate the direct osteogenic effects of hydrogel-derived components, MC3T3-E1 cells were treated with QO or QOMB extracts. QOMB increased Runx2 and Col1A1 fluorescence signals and upregulated osteogenic genes (Alp, Runx2, Col1a1, and Ocn), with the strongest overall response observed in QOMB+ (Fig. S14a–g). These results indicate that QOMB and NIR treatment can promote osteogenic marker expression independently of Schwann cell-mediated paracrine signaling. To determine whether hydrogel-regulated neurotrophic signaling in SCs influenced osteogenic differentiation, conditioned media generated from RSC96 cells under the different treatment conditions were applied to MC3T3-E1 cultures. The osteogenic response was subsequently assessed by ALP and ARS staining. QOMB-conditioned medium produced stronger ALP activity and more extensive calcium deposition than conditioned medium derived from the QO group. In contrast, osteogenic staining remained comparable between the QO and control groups (Fig. 6a and b and Fig. S15). These findings were consistent with the limited effect of QO on neurotrophic factor expression by SCs. Following NIR treatment, the QO+ and QOMB + groups exhibited greater osteogenic activity than their corresponding nonirradiated groups, indicating an additional osteogenic response associated with NIR exposure under mild-heating conditions.

Fig. 6.

Fig. 6

Osteogenic differentiation mediated by Schwann cell-conditioned medium. (a) General view and microscopy images of ALP staining of MC3T3-E1 cells after treatment for 7 days. Scale bars in the first and second rows are 2.5 mm and 1 mm, respectively. (b) General view and microscopy images of ARS staining of MC3T3-E1 cells after treatment for 14 days. Scale bars in the first and second rows are 2.5 mm and 1 mm, respectively. (c) Fluorescence images of Runx2 and Col1A1 after treatment for 7 days. Scale bar: 50 μm. (d, e) Relative fluorescence intensity of Runx2 and Col1A1 staining (n = 3). Western blot analysis of osteogenic protein expression after (f) 7 and (g) 14 days of culture. RT-qPCR analysis of mRNA expression levels of (h) Alp, (i) Runx2, (j) Col1A1 and (k) Ocn after 7 days of different treatments of MC3T3-E1 cells (n = 3). Data are presented as means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001.

These findings were corroborated by IF staining and WB (Fig. 6c–g, Fig. S16 and Fig. S17). MC3T3-E1 cells exposed to QOMB-conditioned medium exhibited higher levels of Col1A1, Runx2, Ocn, and ALP than control groups, and these osteogenic markers were further upregulated following NIR irradiation. RT-qPCR results were consistent with the protein-level findings and suggested that Mn-BGN-induced Schwann cell secretion contributed to the upregulation of osteogenic genes in MC3T3-E1 cells (Fig. 6h–k). Importantly, neutralization of BDNF, GDNF, or NGF in QOMB-conditioned medium attenuated Runx2/Col1A1 protein signals and osteogenic gene expression (Fig. S18), providing loss-of-function evidence that Schwann-cell neurotrophic factors contribute to the paracrine osteogenic response. Additional component-control experiments showed that conditioned media from BGN- or Mn-treated RSC96 cells also enhanced osteogenic markers in MC3T3-E1 cells (Fig. S19), indicating that BGN-derived cues and Mn can modulate the osteogenic activity of the Schwann-cell secretome. Conditioned medium from QOMB + LY294002-treated RSC96 cells reduced Runx2, Col1A1, Alp, and Ocn expression in MC3T3-E1 cells, whereas SC79 rescue in RSC96 cells partially restored these osteogenic readouts. These results indicate that QOMB indirectly promotes osteogenesis through PI3K/AKT activation in Schwann cells (Fig. S20).

To understand the mechanism of how conditioned media from QOMB-treated SCs increase osteogenic differentiation, RNA-seq was performed on MC3T3-E1 cells cultured with conditioned media derived from QOMB- or QO-treated RSC96 cells (Fig. S21). Transcriptomic comparison identified 427 upregulated and 863 downregulated genes in the QOMB-treated group (Fig. S21a). GO analysis highlighted cell migration, cell adhesion, and bone mineralization among the processes enriched in the upregulated gene set, whereas the downregulated DEGs were linked to hypoxic and inflammatory responses (Fig. S21b and c). KEGG analysis additionally demonstrated activation of the TGF-β and PI3K/AKT pathways, accompanied by suppression of osteoclast differentiation and inflammation-related pathways (Fig. S21d and e). GSEA demonstrated negative enrichment of osteoclast differentiation in the QOMB group (Fig. S21f). These transcriptomic findings further supported the involvement of Schwann cell-mediated paracrine signaling in osteogenic differentiation. Together with the direct-extract experiments, these results suggest that QOMB promotes osteogenic responses through both direct material-derived stimulation and Schwann cell-mediated neurotrophic signaling, with the latter further supported by neurotrophic factor neutralization and PI3K/AKT inhibition–rescue experiments. Extract-based cultures and CM transfer have been used to investigate comparable soluble-cue and paracrine mechanisms in biomaterials research [63], [64]. Although the present relay involved rat RSC96 and mouse MC3T3-E1 cells, the two cell types were cultured separately, and similar mixed-species Schwann-cell-CM models have been reported [65]. The conservation of neurotrophic signaling among mammals [66], together with our functional neutralization results, provides further support for this experimental approach. Validation using species-matched primary cells and 3D culture models would extend these findings to a more physiologically representative setting.

3.8. In vivo bone regeneration

The in vivo performance of QOMB combined with sequential PTT was subsequently assessed in a rat model of infected femoral condyle defects, following its antibacterial, immunomodulatory, and neurotrophic effects observed in vitro (Fig. 7a). During the first 3 days after treatment, PTT at 45-50 °C was applied to rapidly control bacterial infection. Thereafter, the PTT temperature was maintained at 40-42 °C to support inflammation resolution and bone repair. Real-time temperature profiles confirmed that the two target windows could be reached and maintained in vivo (Fig. S22). The estimated single-session CEM43 values, calculated from defect-surface temperature profiles over the initial heating period and subsequent 10 min of target-temperature maintenance, were 247.09 min for the antibacterial phase and 0.91 min for the mild-heating phase (Fig. S22). To assess potential thermal injury during the early antibacterial phase, H&E and TUNEL staining were performed on bone defect tissues collected after three consecutive treatment sessions. Comparable histological appearances and TUNEL staining patterns were observed in the Control, NIR, QOMB, and QOMB + groups, without an appreciable increase in local tissue injury in QOMB+ (Fig. S23). These findings suggest that the early treatment did not produce detectable additional histological damage in the examined regions at day 3. Early quantitative colony counting showed a marked reduction in local bacterial burden after hydrogel treatment, with the lowest viable counts in QOMB + group (Fig. S24), supporting the infection-control effect of the staged photothermal protocol. Skeletal healing was examined by micro-CT at 4 and 8 weeks following hydrogel implantation using femoral condyle specimens collected from each group.

Fig. 7.

Fig. 7

In vivo bone regeneration of infected femoral defects by different hydrogels without/with NIR irradiation. (a) Scheme of the animal experiment processes. (b) Micro-CT images of infected bone defect at 4 and 8 weeks after implantation. Scale bar: 2 mm. Quantitative analysis of (c) BV/TV, (d) Tb.N, (e) Tb.Th, and (f) Tb.Sp in implant sites with different treatments (n = 3). (g) H&E and Masson's trichrome staining of the implant sites. Scale bar: 2 mm. Data are presented as means ± SD, *p < 0.05, **p < 0.01, ***p < 0.001, ****p < 0.0001.

Compared with the untreated control, all hydrogel-treated animals revealed better defect healing capability, which might be attributed to the innate antimicrobial and immune modulatory function of the QO hydrogel matrix (Fig. 7b). Compared with QO, QOMB produced more pronounced defect repair, consistent with the combined contribution of Mn-BGN-derived ionic cues, immune remodeling, Schwann-cell-associated neurotrophic signaling, and enhanced osteogenic activity. In addition, NIR-treated groups exhibited smaller residual defects than their nonirradiated counterparts, supporting the regenerative benefit of the staged hydrogel-NIR treatment. This improvement may reflect photothermal stimulation together with potential nonthermal biological effects of 808 nm irradiation.

Micro-CT quantification demonstrated that QOMB + group exhibited the most favorable trabecular parameters, with the highest BV/TV, Tb.N, and Tb.Th, together with the lowest Tb.Sp, reflecting more advanced structural reconstruction within the defect (Fig. 7c–f). Comparable patterns were observed histologically, where the hydrogel-treated groups exhibited smaller residual defect areas and more abundant newly formed bone surrounding the defects (Fig. 7g). To assess whether these structural improvements were coupled with enhanced osteogenic activity, Runx2 and Ocn expression in tissues adjacent to the defects was examined by IF staining (Fig. 8a and b). The QOMB + group exhibited the strongest Runx2 and Ocn signals, consistent with its superior bone-regenerative performance. Bmp2 staining provided additional osteogenic evidence and showed the same trend as Runx2/Ocn and structural regeneration (Fig. S25a, Fig. S26 and S27).

Fig. 8.

Fig. 8

In vivo osteogenic, Schwann-cell-associated neurotrophic, and immune microenvironments. (a) Fluorescence images of Runx2 (red: Runx2, blue: DAPI) at 4 and 8 weeks after implantation. Scale bar: 20 μm. (b) Fluorescence images of Ocn (red: Ocn, blue: DAPI) at 4 and 8 weeks after implantation. Scale bar: 20 μm. Fluorescence images of S100β/BDNF (red: S100β, green: BDNF, blue: DAPI) at (c) 4 and (d) 8 weeks after implantation. Scale bar: 20 μm. Fluorescence images of CD68/CD86/CD206 (white: CD68, red: CD86, green: CD206, blue: DAPI) at (e) 4 and (f) 8 weeks after implantation. Scale bar: 30 μm.

3.9. In vivo neurotrophic and immunomodulatory effects

Peripheral nerves and Schwann cells are widely distributed throughout bone tissue, where they localize within the periosteum, bone marrow, and perivascular regions [67]. The 4- and 8-week time points were selected to align the assessment of neural and inflammatory markers with micro-CT and histological evaluation of bone regeneration and to examine their association with ongoing tissue repair. Given the potential neurotoxicity associated with excessive or sustained Mn exposure, we first examined local Mn retention and systemic biosafety after QOMB implantation. S100β/TUNEL co-staining at 4 and 8 weeks showed only limited TUNEL-positive signals associated with S100β-positive Schwann cells, with no apparent increase in Schwann-cell-associated apoptosis in the QOMB or QOMB + groups (Fig. S28a). Total Mn in defect-associated bone was initially higher in QOMB + than in QOMB and decreased markedly by day 14 in both groups (Fig. S28b). Blood total Mn showed no progressive accumulation during the same period, and H&E staining of major organs revealed no treatment-related histopathological abnormalities (Fig. S29). Because Schwann cell-derived neurotrophic factors contribute to bone repair, BDNF and NGF expression within the defect region was examined by S100β/BDNF and S100β/NGF double staining at weeks 4 and 8 (Fig. 8, 25–27). And thresholded Manders M2 analysis was used to quantify the fraction of neurotrophic-factor signal overlapping S100β-positive structures (Fig. S30). The untreated defects displayed the weakest staining for both neurotrophic factors, in parallel with their poor regenerative outcome (Fig. 8, 25–27). In contrast, the QOMB + group exhibited the highest BDNF and NGF levels. NF200 staining also showed greater neural ingrowth in the QOMB-containing groups (Fig. S25b, S26h and S27h). These findings demonstrated that QOMB promoted the establishment of a Schwann-cell-associated neurotrophic microenvironment at the infected defect area. Concurrently, the antibacterial and immunomodulatory effects of staged NIR treatment created a local milieu favorable for Schwann cell migration and functional activation. Although these results support enhanced neural ingrowth, functional recovery of local nerves was not directly assessed, as the present study focused on Schwann-cell-mediated regulation of bone regeneration rather than nerve-function restoration.

Local IME is another key component of bone repair. IF staining demonstrated that untreated defects displayed strong CD86 staining accompanied by weak CD206 signals, reflecting the persistence of an inflammatory microenvironment following bacterial infection (Fig. 8e, f, Figs. S26 and S27). In contrast, the QOMB + group indicated considerably reduced CD86 expression together with enhanced CD206 staining, suggesting a shift in macrophage phenotype toward a reparative state and the establishment of a pro-regenerative IME. These findings further demonstrated the capacity of QOMB combined with NIR treatment to regulate local immune responses in vivo and create conditions conducive to tissue repair. Taken together, QOMB promoted infected bone regeneration through coordinated antibacterial, immunomodulatory, neural, and osteogenic regulation. Suppression of bacterial burden and remodeling of the inflammatory microenvironment created favorable conditions for tissue repair, while increased Schwann-cell-associated neurotrophic signals and neural ingrowth paralleled enhanced osteogenic marker expression and bone formation. These findings support a cooperative regenerative mechanism in which neuro-osteogenic coupling functions together with infection control and immune remodeling to promote bone repair. Although the micro-CT, osteogenic, neurotrophic, and inflammatory findings consistently supported the proposed repair-associated responses, the relatively small animal cohort limited the precision of effect estimates. Further validation in larger, independent cohorts will help establish the robustness and reproducibility of the observed therapeutic effects.

4. Conclusions

In this study, we engineered an NIR-responsive hydrogel (QOMB) by incorporating Mn-BGN into a dynamic gallic acid-functionalized chitosan-alginate network. QOMB combined contact-active antibacterial chemistry with NIR-triggered heating and reduced both planktonic bacterial viability and established biofilm biomass. Mn-BGN-associated dissolution products modulated macrophage and Schwann-cell responses. In RSC96 cells, inhibition-rescue experiments supported a functional PI3K/AKT-CREB contribution to BDNF/NGF regulation, and neutralization experiments showed that Schwann-cell-derived neurotrophic factors contribute to the osteogenic activity of conditioned medium. In vivo, QOMB combined with staged NIR treatment reduced early bacterial burden, improved structural bone regeneration, and was accompanied by increased NF200-positive neural structures and S100β-associated BDNF/NGF signals. These findings establish a temporally coordinated infection-control and neuro-osteogenic regeneration strategy rather than relying on the individual novelty of the constituent materials. The present study remains limited by the small-animal model, mixed-species cell-line system, absence of direct angiogenesis testing, and incomplete resolution of the independent roles of Mn, Si, and Ca. Further work in species-matched 3D models and larger animals will be required for translational validation.

CRediT authorship contribution statement

Xinkai Cui: Writing – original draft, Methodology, Investigation, Data curation, Conceptualization. Junxian Ma: Investigation, Data curation. Zhenyu Yang: Methodology. Huiwen Luo: Methodology, Conceptualization. Shiqi Dai: Methodology, Investigation. Kai Tang: Methodology. Wen Niu: Writing – review & editing, Project administration, Methodology, Conceptualization. Jihua Chen: Supervision, Resources, Project administration, Funding acquisition, Conceptualization. Lina Niu: Supervision, Resources, Project administration, Conceptualization.

Data availability

The datasets generated in this study are available from the corresponding author upon reasonable request.

Ethics approval and consent to participate

All animal procedures were approved by the Experimental Animal Welfare and Ethics Committee of the Hospital of Stomatology, Fourth Military Medical University (permission no. IACUC-2025-kq-071).

Declaration of competing interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Acknowledgments

This work was supported by the National Natural Science Foundation of China (Grant No. 82370994). Figure support for graphical abstract was provided by BioRender.com.

Footnotes

Peer review under the responsibility of editorial board of Bioactive Materials.

Appendix A

Supplementary data to this article can be found online at https://doi.org/10.1016/j.bioactmat.2026.10.039.

Contributor Information

Wen Niu, Email: niuwen9302@fmmu.edu.cn.

Jihua Chen, Email: jhchen@fmmu.edu.cn.

Lina Niu, Email: niulina831013@126.com.

Appendix A. Supplementary data

The following are the Supplementary data to this article.

Multimedia component 1
mmc1.docx (46.5MB, docx)
Multimedia component 2
mmc2.pdf (1.9MB, pdf)

References

  • 1.Kim H.D., Amirthalingam S., Kim S.L., Lee S.S., Rangasamy J., Hwang N.S. Biomimetic materials and fabrication approaches for bone tissue engineering. Adv. Healthc. Mater. 2017;6 doi: 10.1002/adhm.201700612. [DOI] [PubMed] [Google Scholar]
  • 2.Yang Y., Chu L., Yang S., Zhang H., Qin L., Guillaume O., Eglin D., Richards R.G., Tang T. Dual-functional 3D-printed composite scaffold for inhibiting bacterial infection and promoting bone regeneration in infected bone defect models. Acta Biomater. 2018;79:265–275. doi: 10.1016/j.actbio.2018.08.015. [DOI] [PubMed] [Google Scholar]
  • 3.Behzadi S., Luther G.A., Harris M.B., Farokhzad O.C., Mahmoudi M. Nanomedicine for safe healing of bone trauma: opportunities and challenges. Biomaterials. 2017;146:168–182. doi: 10.1016/j.biomaterials.2017.09.005. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 4.Li X., Yang Y., Chen M., Liu X., Chen T., Luo F., Huang Y., Liu Y., Zhang H., Chen S., Bai D., Ding C., Li J. Diatom-inspired scaffold for infected bone defect therapy: achieving stable photothermal properties and coordinated antibacterial-osteogenic functions. Adv. Mater. 2026;38 doi: 10.1002/adma.202509997. [DOI] [PubMed] [Google Scholar]
  • 5.Mei Z., Gao D., Hu D., Zhou H., Ma T., Huang L., Liu X., Zheng R., Zheng H., Zhao P., Zhou J., Sheng Z. Activatable NIR-II photoacoustic imaging and photochemical synergistic therapy of MRSA infections using miniature Au/Ag nanorods. Biomaterials. 2020;251 doi: 10.1016/j.biomaterials.2020.120092. [DOI] [PubMed] [Google Scholar]
  • 6.Wu Y., Xie X., Luo G., Xie J., Ye X., Gu W., Mo A., Qian Z., Zhou C., Liao J. Photothermal sensitive nanocomposite hydrogel for infectious bone defects. Bone Res. 2025;13:22. doi: 10.1038/s41413-024-00377-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 7.Chen H., Hu B., Lv X., Zhu S., Zhen G., Wan M., Jain A., Gao B., Chai Y., Yang M., Wang X., Deng R., Wang L., Cao Y., Ni S., Liu S., Yuan W., Chen H., Dong X., Guan Y., Yang H., Cao X. Prostaglandin E2 mediates sensory nerve regulation of bone homeostasis. Nat. Commun. 2019;10:181. doi: 10.1038/s41467-018-08097-7. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 8.Wan Q., Qin W., Ma Y., Shen M., Li J., Zhang Z., Chen J., Tay F.R., Niu L., Jiao K. Crosstalk between bone and nerves within bone. Adv. Sci. 2021;8 doi: 10.1002/advs.202003390. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 9.Tao R., Mi B., Hu Y., Lin S., Xiong Y., Lu X., Panayi A.C., Li G., Liu G. Hallmarks of peripheral nerve function in bone regeneration. Bone Res. 2023;11:6. doi: 10.1038/s41413-022-00240-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 10.Li Z., Meyers C.A., Chang L., Lee S., Li Z., Tomlinson R., Hoke A., Clemens T.L., James A.W. Fracture repair requires TrkA signaling by skeletal sensory nerves. J. Clin. Investig. 2019;129:5137–5150. doi: 10.1172/JCI128428. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 11.Fukuda T., Takeda S., Xu R., Ochi H., Sunamura S., Sato T., Shibata S., Yoshida Y., Gu Z., Kimura A., Ma C., Xu C., Bando W., Fujita K., Shinomiya K., Hirai T., Asou Y., Enomoto M., Okano H., Okawa A., Itoh H. Sema3A regulates bone-mass accrual through sensory innervations. Nature. 2013;497:490–493. doi: 10.1038/nature12115. [DOI] [PubMed] [Google Scholar]
  • 12.Sun W., Ye B., Chen S., Zeng L., Lu H., Wan Y., Gao Q., Chen K., Qu Y., Wu B., Lv X., Guo X. Neuro–bone tissue engineering: emerging mechanisms, potential strategies, and current challenges. Bone Res. 2023;11:65. doi: 10.1038/s41413-023-00302-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 13.Li X.-L., Zhao Y.-Q., Miao L., An Y.-X., Wu F., Han J.-Y., Han J.-Y., Tay F.R., Mu Z., Jiao Y., Wang J. Strategies for promoting neurovascularization in bone regeneration. Mil. Med. Res. 2025;12:9. doi: 10.1186/s40779-025-00596-1. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 14.Xu M., Li Z., Thottappillil N., Cherief M., Zhu M., Xing X., Gomez-Salazar M., Rao C., Ramesh S., Mwirigi J.M., Sankaranarayanan I., Tavares-Ferreira D., Zhang C., Wang X.-W., Archer M., Guan Y., Tower R.J., Cahan P., Price T.J., Clemens T.L., James A.W. Mapping somatosensory afferent circuitry to bone identifies neurotrophic signals required for fracture healing. Science. 2026;391 doi: 10.1126/science.adr9608. [DOI] [PubMed] [Google Scholar]
  • 15.Arthur-Farraj P.J., Latouche M., Wilton D.K., Quintes S., Chabrol E., Banerjee A., Woodhoo A., Jenkins B., Rahman M., Turmaine M., Wicher G.K., Mitter R., Greensmith L., Behrens A., Raivich G., Mirsky R., Jessen K.R. c-Jun reprograms schwann cells of injured nerves to generate a repair cell essential for regeneration. Neuron. 2012;75:633–647. doi: 10.1016/j.neuron.2012.06.021. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 16.Clements M.P., Byrne E., Camarillo Guerrero L.F., Cattin A.-L., Zakka L., Ashraf A., Burden J.J., Khadayate S., Lloyd A.C., Marguerat S., Parrinello S. The wound microenvironment reprograms schwann cells to invasive mesenchymal-like cells to drive peripheral nerve regeneration. Neuron. 2017;96:98–114.e7. doi: 10.1016/j.neuron.2017.09.008. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 17.Shen X., Zhang H., Song Z., Dong Y., Ge X., Jin S., Guo S., Zhang P., Fu Y., Zhu Y., Xiao N., Wang D., Cheng J., Xu R., Jiang H. Enhancer-driven shh signaling promotes glia-to-mesenchyme transition during bone repair. Bone Res. 2025;13:16. doi: 10.1038/s41413-024-00396-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 18.Cattin A.-L., Burden J.J., Van Emmenis L., Mackenzie F.E., Hoving J.J.A., Garcia Calavia N., Guo Y., McLaughlin M., Rosenberg L.H., Quereda V., Jamecna D., Napoli I., Parrinello S., Enver T., Ruhrberg C., Lloyd A.C. Macrophage-induced blood vessels guide schwann cell-mediated regeneration of peripheral nerves. Cell. 2015;162:1127–1139. doi: 10.1016/j.cell.2015.07.021. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 19.Parrinello S., Napoli I., Ribeiro S., Digby P.W., Fedorova M., Parkinson D.B., Doddrell R.D.S., Nakayama M., Adams R.H., Lloyd A.C. EphB signaling directs peripheral nerve regeneration through Sox2-dependent schwann cell sorting. Cell. 2010;143:145–155. doi: 10.1016/j.cell.2010.08.039. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 20.Xu J., Li Z., Tower R.J., Negri S., Wang Y., Meyers C.A., Sono T., Qin Q., Lu A., Xing X., McCarthy E.F., Clemens T.L., James A.W. NGF-p75 signaling coordinates skeletal cell migration during bone repair. Sci. Adv. 2022;8 doi: 10.1126/sciadv.abl5716. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 21.Hao Z., Ren L., Zhang Z., Yang Z., Wu S., Liu G., Cheng B., Wu J., Xia J. A multifunctional neuromodulation platform utilizing schwann cell-derived exosomes orchestrates bone microenvironment via immunomodulation, angiogenesis and osteogenesis. Bioact. Mater. 2023;23:206–222. doi: 10.1016/j.bioactmat.2022.10.018. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 22.Cai X., Luo E., Yuan Q. Interaction between schwann cells and osteoblasts in vitro. Int. J. Oral Sci. 2010;2:74–81. doi: 10.4248/IJOS10039. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 23.Bi C., Fu Y., Li B. Brain-derived neurotrophic factor alleviates diabetes mellitus-accelerated atherosclerosis by promoting M2 polarization of macrophages through repressing the STAT3 pathway. Cell. Signal. 2020;70 doi: 10.1016/j.cellsig.2020.109569. [DOI] [PubMed] [Google Scholar]
  • 24.Zhu W., Jin L., Zhang Q., Cui Y., Zou Y., Chen P., Ye J., Xiong Y., Lin M., Zhou Y., Wu R., Liang Y., Zhuang Z., Huh J.Y., Luo W., Liang G. Brain-derived neurotrophic factor and the derived dodecapeptide function as toll-like receptor 4 antagonists in acute lung injury. Nat. Commun. 2026;17:2786. doi: 10.1038/s41467-026-69541-7. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 25.Zhu W., Cui Y., Zhou Y., Zheng Y., Huang L., Jin L., Zhang Q., Chen P., Lin M., Ye J., Xiong Y., Huh J.Y., Hu X., Li X., Luo W., Liang G. Hepatocyte BDNF acts as a novel immune checkpoint to restrain TLR4-mediated acute hepatitis. Adv. Sci. 2026;13 doi: 10.1002/advs.202521164. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 26.Emanueli C., Salis M.B., Pinna A., Graiani G., Manni L., Madeddu P. Nerve growth factor promotes angiogenesis and arteriogenesis in ischemic hindlimbs. Circulation. 2002;106:2257–2262. doi: 10.1161/01.CIR.0000033971.56802.C5. [DOI] [PubMed] [Google Scholar]
  • 27.Wang X., Yu Y., Zhang R., Xu J., Kang Q. Enhanced bone regeneration by schwann cells through coupling of osteogenesis and angiogenesis via β-catenin signaling in a preclinical model of distraction osteogenesis. Int. J. Med. Sci. 2025;22:209–226. doi: 10.7150/ijms.100854. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 28.Tian J., Zhao Y., Zhang Q., Li S., Luo M., Chen M., Huang Q., Lei B. SOD/CAT-biomimetic bioactive glass-ceramics nanozyme with intracellular oxygen supply and immunoregulation for MRSA-infected wound repair. Chem. Eng. J. 2025;513 doi: 10.1016/j.cej.2025.162671. [DOI] [Google Scholar]
  • 29.Liu X., Shen M., Bing T., Zhang X., Li Y., Cai Q., Yang X., Yu Y. A bioactive injectable hydrogel regulates tumor metastasis and wound healing for melanoma via NIR-light triggered hyperthermia. Adv. Sci. 2024;11 doi: 10.1002/advs.202402208. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 30.Yin Y., Cai Y., Dang P., Zeng W., Wang L., Yan X., Luo Z., Liu W., Zhu Y., Chen L., Zhang C. A near-infrared regulated programmable multi-mode periosteum scaffold for sequential healing of infected bone defects. Bioact. Mater. 2026;63:56–72. doi: 10.1016/j.bioactmat.2026.03.046. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 31.Tang J., Hu J., Bai X., Wang Y., Cai J., Zhang Z., Geng B., Pan D., Shen L. Near-infrared carbon dots with antibacterial and osteogenic activities for sonodynamic therapy of infected bone defects. Small. 2024;20 doi: 10.1002/smll.202404900. [DOI] [PubMed] [Google Scholar]
  • 32.Zorrón M., Cabrera A.L., Sharma R., Radhakrishnan J., Abbaszadeh S., Shahbazi M., Tafreshi O.A., Karamikamkar S., Maleki H. Emerging 2D nanomaterials-integrated hydrogels: advancements in designing theragenerative materials for bone regeneration and disease therapy. Adv. Sci. 2024;11 doi: 10.1002/advs.202403204. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 33.Zeng J., Gu C., Geng X., Lin K., Xie Y., Chen X. Combined photothermal and sonodynamic therapy using a 2D black phosphorus nanosheets loaded coating for efficient bacterial inhibition and bone-implant integration. Biomaterials. 2023;297 doi: 10.1016/j.biomaterials.2023.122122. [DOI] [PubMed] [Google Scholar]
  • 34.Xu T., Hua Y., Mei P., Zeng D., Jiang S., Liao C. Black phosphorus thermosensitive hydrogels loaded with bone marrow mesenchymal stem cell-derived exosomes synergistically promote bone tissue defect repair. J. Mater. Chem. B. 2023;11:4396–4407. doi: 10.1039/D3TB00341H. [DOI] [PubMed] [Google Scholar]
  • 35.Su J., Liang X., Yang J., Dong X., Chen Y., Tan X., Li Z., Song Y., Zhang H., Dai H., Yu A. Mild photothermal-responsive hydrogel with H2Se delivery for anti-infection and microenvironment remodeling to bone regeneration in diabetic osteomyelitis. Bioact. Mater. 2026;64:159–179. doi: 10.1016/j.bioactmat.2026.04.041. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 36.Fan Y., Zhai J., Wang Z., Yin Z., Chen H., Ran M., Zhu Z., Ma Y., Ning C., Yu P., Mao C. Piezoelectric heterojunctions as bacteria-killing bone-regenerative implants. Adv. Mater. 2025;37 doi: 10.1002/adma.202413171. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 37.Huang Y., Li J., Yu Z., Li J., Liang K., Deng Y. Elaborated bio-heterojunction with robust sterilization effect for infected tissue regeneration via activating competent cell-like antibacterial tactic. Adv. Mater. 2024;36 doi: 10.1002/adma.202414111. [DOI] [PubMed] [Google Scholar]
  • 38.Li J., Deng C., Liang W., Kang F., Bai Y., Ma B., Wu C., Dong S. Mn-containing bioceramics inhibit osteoclastogenesis and promote osteoporotic bone regeneration via scavenging ROS. Bioact. Mater. 2021;6:3839–3850. doi: 10.1016/j.bioactmat.2021.03.039. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 39.Sabino R.M., Rau J.V., De Bonis A., De Stefanis A., Curcio M., Teghil R., Popat K.C. Manganese-containing bioactive glass enhances osteogenic activity of TiO2 nanotube arrays. Appl. Surf. Sci. 2021;570 doi: 10.1016/j.apsusc.2021.151163. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 40.Briggs D.C., Hohenester E. Structural basis for the initiation of glycosaminoglycan biosynthesis by human xylosyltransferase 1. Structure. 2018;26:801–809.e3. doi: 10.1016/j.str.2018.03.014. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 41.Khan S., Sbeity M., Foulquier F., Barré L., Ouzzine M. TMEM165 a new player in proteoglycan synthesis: loss of TMEM165 impairs elongation of chondroitin- and heparan-sulfate glycosaminoglycan chains of proteoglycans and triggers early chondrocyte differentiation and hypertrophy. Cell Death Dis. 2022;13:11. doi: 10.1038/s41419-021-04458-1. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 42.Tan C.L., Kwok J.C.F., Patani R., ffrench-Constant C., Chandran S., Fawcett J.W. Integrin activation promotes axon growth on inhibitory chondroitin sulfate proteoglycans by enhancing integrin signaling. J. Neurosci. 2011;31:6289–6295. doi: 10.1523/JNEUROSCI.0008-11.2011. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 43.Li L., Xiao B., Mu J., Zhang Y., Zhang C., Cao H., Chen R., Patra H.K., Yang B., Feng S., Tabata Y., Slater N.K.H., Tang J., Shen Y., Gao J. A MnO nanoparticle-dotted hydrogel promotes spinal cord repair via regulating reactive oxygen species microenvironment and synergizing with mesenchymal stem cells. ACS Nano. 2019;13:14283–14293. doi: 10.1021/acsnano.9b07598. [DOI] [PubMed] [Google Scholar]
  • 44.Peres T.V., Schettinger M.R.C., Chen P., Carvalho F., Avila D.S., Bowman A.B., Aschner M. Manganese-induced neurotoxicity: a review of its behavioral consequences and neuroprotective strategies. BMC Pharmacol. Toxicol. 2016;17:57. doi: 10.1186/s40360-016-0099-0. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 45.Li L., Qin W., Ye T., Wang C., Qin Z., Ma Y., Mu Z., Jiao K., Tay F.R., Niu W., Niu L. Bioactive zn–v–si–ca glass nanoparticle hydrogel microneedles with antimicrobial and antioxidant properties for bone regeneration in diabetic periodontitis. ACS Nano. 2025;19:7981–7995. doi: 10.1021/acsnano.4c15227. [DOI] [PubMed] [Google Scholar]
  • 46.Du L., Wu J., Han Y., Wu C. Immunomodulatory multicellular scaffolds for tendon-to-bone regeneration. Sci. Adv. 2024;10 doi: 10.1126/sciadv.adk6610. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 47.Sun Y., Zhang H., Zhang Y., Liu Z., He D., Xu W., Li S., Zhang C., Zhang Z. Li–Mg–Si bioceramics provide a dynamic immuno-modulatory and repair-supportive microenvironment for peripheral nerve regeneration. Bioact. Mater. 2023;28:227–242. doi: 10.1016/j.bioactmat.2023.05.013. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 48.Tao X., Zhang H., Mei P., Huang J., Fang B., Huan Z., Wu C. An injectable bioceramics-containing composite hydrogel promoting innervation for pulp-dentin complex repair. Int. J. Oral Sci. 2025;17:66. doi: 10.1038/s41368-025-00398-0. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 49.Zhao D., Wang X., Cheng B., Yin M., Hou Z., Li X., Liu K., Tie C., Yin M. Degradation-kinetics-controllable and tissue-regeneration-matchable photocross-linked alginate hydrogels for bone repair. ACS Appl. Mater. Interfaces. 2022;14:21886–21905. doi: 10.1021/acsami.2c01739. [DOI] [PubMed] [Google Scholar]
  • 50.Shan Y., Cao F., Zhao X., Luo J., Mei H., Zhang L., Huang Y., Yang Y., Yan L., Huang Y., Han Y., Guo B. Procoagulant, antibacterial and antioxidant high-strength porous hydrogel adhesives in situ formed via self-gelling hemostatic microsheets for emergency hemostasis and wound repair. Biomaterials. 2025;315 doi: 10.1016/j.biomaterials.2024.122936. [DOI] [PubMed] [Google Scholar]
  • 51.Zhao X., Huang Y., Li Z., Chen J., Luo J., Bai L., Huang H., Cao E., Yin Z., Han Y., Guo B. Injectable self-expanding/self-propelling hydrogel adhesive with procoagulant activity and rapid gelation for lethal massive hemorrhage management. Adv. Mater. 2024;36 doi: 10.1002/adma.202308701. [DOI] [PubMed] [Google Scholar]
  • 52.Hou X., Zhang L., Chen Y., Liu Z., Zhao X., Lu B., Luo Y., Qu X., Musskaya O., Glazov I., Kulak A.I., Chen F., Zhao J., Zhou Z., Zheng L. Photothermal switch by gallic acid-calcium grafts synthesized by coordination chemistry for sequential treatment of bone tumor and regeneration. Biomaterials. 2025;312 doi: 10.1016/j.biomaterials.2024.122724. [DOI] [PubMed] [Google Scholar]
  • 53.Chen J., Xian G., Xiao Z., Ge F., Yuan S., Li B., Liang X., Cai Z., Zhang N., Zhang L., Li Z.A., Deng L., Zeng C., Xie D. Biomineralization-inspired scaffolds using citrate-based polymers to stabilize amorphous calcium phosphate promote osteogenesis and angiogenesis for bone defect repair. Bioact. Mater. 2026;56:260–276. doi: 10.1016/j.bioactmat.2025.10.016. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 54.Li Z., He D., Guo B., Wang Z., Yu H., Wang Y., Jin S., Yu M., Zhu L., Chen L., Ding C., Wu X., Wu T., Gong S., Mao J., Zhou Y., Luo D., Liu Y. Self-promoted electroactive biomimetic mineralized scaffolds for bacteria-infected bone regeneration. Nat. Commun. 2023;14:6963. doi: 10.1038/s41467-023-42598-4. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 55.Liu J., Wei J., Xiao S., Yuan L., Liu H., Zuo Y., Li Y., Li J. Multienzyme-activity sulfur quantum dot nanozyme-mediated cascade reactions in whole-stage symptomatic therapy of infected bone defects. ACS Nano. 2025;19:6858–6875. doi: 10.1021/acsnano.4c12343. [DOI] [PubMed] [Google Scholar]
  • 56.Bôle M., Amouzou K.D., Gaucher V., Degoutin S., Benbettaieb N., Debeaufort F. Influence of annealing and crosslinking on release properties of gallic acid from polyvinyl alcohol-based films for packaging applications. Food Hydrocoll. 2026;179 doi: 10.1016/j.foodhyd.2026.112793. [DOI] [Google Scholar]
  • 57.Li P., Poon Y.F., Li W., Zhu H.-Y., Yeap S.H., Cao Y., Qi X., Zhou C., Lamrani M., Beuerman R.W., Kang E.-T., Mu Y., Li C.M., Chang M.W., Jan Leong S.S., Chan-Park M.B. A polycationic antimicrobial and biocompatible hydrogel with microbe membrane suctioning ability. Nat. Mater. 2011;10:149–156. doi: 10.1038/nmat2915. [DOI] [PubMed] [Google Scholar]
  • 58.Cheng Z., Kang M., Peng X., Ren L., Xie J., Yuan Q., Xu X., Li J. Self-assembled eutectogel with cell permeation and multiple anti-inflammatory abilities for treating chronic periodontitis. Adv. Mater. 2025;37 doi: 10.1002/adma.202412866. [DOI] [PubMed] [Google Scholar]
  • 59.Cometta S., Donose B.C., Juárez-Saldivar A., Ravichandran A., Xu Y., Bock N., Dargaville T.R., Rakić A.D., Hutmacher D.W. Unravelling the physicochemical and antimicrobial mechanisms of human serum albumin/tannic acid coatings for medical-grade polycaprolactone scaffolds. Bioact. Mater. 2024;42:68–84. doi: 10.1016/j.bioactmat.2024.08.023. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 60.Yao X., Kong L., Qiao Y., Brand D., Li J., Yan Z., Zheng S.G., Qian Y., Fan C. Schwann cell-secreted frizzled-related protein 1 dictates neuroinflammation and peripheral nerve degeneration after neurotrauma. Cell Rep. Med. 2024;5 doi: 10.1016/j.xcrm.2024.101791. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 61.Yang J., Shuai J., Siow L., Lu J., Sun M., An W., Yu M., Wang B., Chen Q. MicroRNA-146a-loaded magnesium silicate nanospheres promote bone regeneration in an inflammatory microenvironment. Bone Res. 2024;12:2. doi: 10.1038/s41413-023-00299-0. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 62.Ou Z., Wei J., Lei J., Wu D., Tong B., Liang H., Zhu D., Wang H., Zhou X., Xu H., Du Z., Du Y., Tan L., Yang C., Feng X. Biodegradable Janus sonozyme with continuous reactive oxygen species regulation for treating infected critical-sized bone defects. Nat. Commun. 2024;15:10525. doi: 10.1038/s41467-024-54894-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 63.Su Q., Wang J., Song Y., Zhang Z., Cai B., Xiaohalati X., Liu J., Li H., Wang Z., Chang J., Wang L. Bioactive silk sericin/bioceramic nerve guidance conduit for effective repair of long-gap transected peripheral nerve injury through regulating schwann cells. Adv. Sci. 2025;12 doi: 10.1002/advs.202507241. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 64.Zhou P., Xia D., Ni Z., Ou T., Wang Y., Zhang H., Mao L., Lin K., Xu S., Liu J. Calcium silicate bioactive ceramics induce osteogenesis through oncostatin M. Bioact. Mater. 2021;6:810–822. doi: 10.1016/j.bioactmat.2020.09.018. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 65.Zhang Q., Gao S., Li B., Li Q., Li X., Cheng J., Peng Z., Liang J., Zhang K., Hai J., Zhang B. Lithium-doped titanium dioxide-based multilayer hierarchical structure for accelerating nerve-induced bone regeneration. ACS Appl. Mater. Interfaces. 2024;16:22887–22899. doi: 10.1021/acsami.4c01520. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 66.Barde Y.-A. The physiopathology of brain-derived neurotrophic factor. Physiol. Rev. 2025;105:2073–2140. doi: 10.1152/physrev.00038.2024. [DOI] [PubMed] [Google Scholar]
  • 67.Gao X., Murphy M.M., Peyer J.G., Ni Y., Yang M., Zhang Y., Guo J., Kara N., Embree C., Tasdogan A., Ubellacker J.M., Crane G.M., Fang S., Zhao Z., Shen B., Morrison S.J. Leptin receptor+ cells promote bone marrow innervation and regeneration by synthesizing nerve growth factor. Nat. Cell Biol. 2023;25:1746–1757. doi: 10.1038/s41556-023-01284-9. [DOI] [PMC free article] [PubMed] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Multimedia component 1
mmc1.docx (46.5MB, docx)
Multimedia component 2
mmc2.pdf (1.9MB, pdf)

Data Availability Statement

The datasets generated in this study are available from the corresponding author upon reasonable request.