Skip to main content
RSC Advances logoLink to RSC Advances
. 2026 Nov 16. Online ahead of print. doi: 10.1039/d6ra08739f

Zn-modified hierarchical ZSM-5 and the role of bimetallic promoters in methanol to aromatic conversion

Arash Abbasi a, Kobra Pourabdollah a,✉, Babak Mokhtarani a
PMCID: PMC13772011  PMID: 43041823

Abstract

A sustainable one-pot synthesis strategy was developed for the preparation of hierarchical Zn-modified ZSM-5 catalysts using polyvinylpyrrolidone (PVP) as an eco-friendly secondary template, while Ni and Cr were introduced as bimetallic promoters to elucidate their roles in catalytic performance and structure–activity relationships during methanol-to-aromatics (MTA) conversion. Catalytic performance was evaluated in the MTA reaction at 400 °C, atmospheric pressure, and a WHSV of 5 h−1, achieving over 99.5% methanol conversion across all samples. Comprehensive physicochemical characterization demonstrated that PVP-assisted synthesis generated an optimized micro–mesoporous architecture, improved Zn and Al incorporation into the zeolite framework, and enhanced accessibility to active sites. XPS analysis revealed a substantial increase in catalytically active Zn (OH)+ species, particularly in Ni-promoted catalysts, indicating superior Zn dispersion and enhanced dehydrogenation functionality. BET, SEM, and NH3-TPD analyses further confirmed that hierarchical structuring improved diffusion properties, external surface area, and acidity balance, leading to superior catalytic efficiency. Among the prepared catalysts, Zn@PVP/ZC exhibited markedly improved aromatic (67.3%) and BTX (61.8%) selectivity, while ZnNi@PVP/ZC delivered the highest BTX selectivity (67.9%), enhanced catalyst stability, and minimized coke formation due to synergistic Zn–Ni interactions. In contrast, Cr promotion increased excessive strong acidity and accelerated internal coke deposition, resulting in reduced catalytic lifetime and lower BTX productivity. Overall, this work establishes a rational and green catalytic design strategy for high-performance hierarchical ZSM-5 catalysts, highlighting the critical role of bimetallic promotion in optimizing methanol aromatization efficiency.


A sustainable one-pot synthesis of hierarchical Zn-modified ZSM-5 catalysts using PVP as an eco-friendly template, with Ni and Cr promoters to investigate structure–activity relationships in methanol-to-aromatics conversion.graphic file with name d6ra08739f-ga.webp

1. Introduction

The growing global demand for aromatic hydrocarbons has intensified interest in developing sustainable and economically viable production technologies. Benzene, toluene, and xylenes (BTX) are among the most important aromatic compounds in the petrochemical industry and serve as essential feedstocks for the manufacture of polymers, synthetic fibers, detergents, pharmaceuticals, agrochemicals, solvents, and numerous specialty chemicals.1,2 Owing to their extensive industrial utilization, the global market for aromatic compounds continues to expand steadily, motivating the search for alternative production routes capable of reducing reliance on conventional petroleum resources.3

Traditionally, aromatic hydrocarbons are produced through petroleum-based processes such as catalytic reforming of naphtha and steam cracking.3,4 However, concerns associated with fossil fuel depletion, fluctuating crude oil prices, and environmental sustainability have stimulated significant research into non-petroleum pathways for aromatic production. Various renewable and alternative feedstocks have been investigated, including biomass-derived intermediates, waste plastics, lignin-rich materials, and alcohol-based feedstocks.5–13 Among these alternatives, methanol has emerged as a particularly attractive platform molecule because it can be synthesized from a broad range of carbon sources, including natural gas, coal, biomass, municipal waste, and carbon dioxide through hydrogenation processes.14–16 This versatility has positioned methanol as a key intermediate within the framework of future sustainable carbon cycles and has stimulated growing interest in methanol-to-aromatics (MTA) technology.

The efficiency of the MTA process is strongly dependent on catalyst characteristics. Among the various catalyst systems investigated, ZSM-5 zeolite has received widespread attention due to its unique MFI framework, strong acidity, hydrothermal stability, and shape-selective properties.17–19 The MFI structure consists of interconnected straight and sinusoidal channels formed by ten-membered oxygen rings, providing a confined environment that favors the formation of aromatic products.20 The shape-selective behavior of ZSM-5 originates from its confined channel system, comprising straight channels (∼5.3 × 5.6 A) intersecting with sinusoidal channels (∼5.1 × 5.5 A).20 These dimensions are comparable to the kinetic diameter of para-xylene (∼5.8 A), which diffuses considerably faster than its bulkier ortho- and meta-isomers (∼6.8 Å) or trimethylbenzenes, resulting in an inherent product-shape selectivity that favors linear, less-branched aromatics and limits the outward diffusion of bulky polymethylated species.21,22 This intrinsic selectivity can be further modulated by acid-site location, external surface passivation, and crystal/particle size.23–25

Nevertheless, the microporous nature of conventional ZSM-5 also introduces significant diffusion limitations. The restricted transport of bulky intermediates and aromatic molecules often promotes secondary reactions, accelerates carbon deposition, and eventually causes catalyst deactivation. As a result, aromatic selectivity and catalyst lifetime are frequently compromised during prolonged operation.26,27

To overcome diffusion-related limitations, considerable efforts have been devoted to the development of hierarchical zeolites containing both microporous and mesoporous networks. The incorporation of mesopores into the zeolite structure improves molecular transport, increases accessibility to active sites, and facilitates the diffusion of reaction products out of the catalyst framework.28

Consequently, hierarchical ZSM-5 catalysts often exhibit enhanced catalytic activity, improved aromatic selectivity, and reduced coke accumulation compared with their purely microporous counterparts. The combination of intrinsic shape selectivity provided by micropores and enhanced mass transfer offered by mesopores makes hierarchical ZSM-5 particularly attractive for industrial MTA applications.29

Strategies to introduce mesoporosity into ZSM-5—post-synthetic desilication/dealumination and bottom-up templating with hard, soft, or green secondary templates—have been reviewed extensively,28–50 and their relative merits and limitations were discussed in detail in our previous comparative study of polymer-templated hierarchical ZSM-5.51 Post-synthetic alkaline treatment is simple but prone to structural damage and uncontrolled Al leaching,29,30 while bottom-up templating with water-soluble polymers such as PVP offers a lower-waste route to uniform, defect-tolerant mesoporosity while preserving crystallinity.51 PVP has previously been shown by our group to outperform PEG in generating uniform, crystallinity-preserving mesoporosity for unmodified ZSM-5 in MTA,51 motivating its selection as the sole secondary template in the present metal-promoted system.

Although hierarchical zeolites effectively reduce mass-transfer limitations and shorten reactant pathways, thereby increasing aromatic selectivity, the results remain suboptimal. This is particularly evident in the selectivity of BTX due to the high formation of alkanes.52

In particular, the selective conversion of methanol-derived intermediates into BTX compounds requires a delicate balance between acidity and dehydrogenation functionality.52 Therefore, metal modification has become a widely adopted strategy for tuning catalytic behavior and enhancing aromatic production.53

Numerous metal species, including Ga, Zn, Ag, La, Cu, Ni, Re, Sn, and Cd, have been incorporated into ZSM-5 catalysts to improve MTA performance.20,54 These metals can facilitate dehydrogenation reactions, promote aromatization pathways, and suppress undesired hydrogen-transfer reactions that lead to excessive alkane formation. Among them, zinc has emerged as one of the most effective and economically attractive promoters due to its abundance, low toxicity, and strong ability to enhance aromatic selectivity. Several studies have reported that Zn-modified ZSM-5 catalysts exhibit superior aromatic yields compared with unmodified zeolites, particularly when zinc species are highly dispersed within the zeolite framework.27,54

Yang et al.,54 using desilicated Zn-modified ZSM-5 in the MTA reaction, report that enhanced mass diffusion within the mesopores, the presence of appropriate acidic sites, and the augmented specific surface area following NaOH treatment resulted in the minimal rate of coke formation and an increased yield of aromatics, rising from 41.3% to 55.3%, from conventional unmodified ZSM-5 to Zn-hierarchical ZSM-5. Liu et al.27 synthesized Zn@ZSM-5 using the dry gel method to encapsulate metal particles within zeolites. This approach is considered an efficient strategy for protecting metal nanoparticles from sintering and exposure to poisonous substrates. They report that this encapsulation method achieves approximately 6% greater aromatic selectivity than the traditional metal-impregnation method used in zeolites. Despite these advantages, Zn-containing catalysts still face challenges related to catalyst deactivation, coke deposition, and limited BTX selectivity. Several approaches have been reported to reduce the coke formation rate and enhance BTX selectivity.10,21,55,56 Researchers developed SiO2 surface passivation of P–Zn/ZSM-5 and utilized it for MTA reaction. They report that passivated samples raise p-xylene selectivity to 90%, but the total aromatic decreases by 15%.21 In another study, this trend was also evident when Mg and P were added to the Zn/ZSM-5 catalyst. This finding indicates a reduction in the catalyst's acidic strength, thereby limiting aromatization reactions.57

Another methodology employs dual-metal promoters that enhance BTX selectivity by utilizing synergistic effects between metals, while maintaining high aromatic selectivity and minimizing coke formation. Vicente et al.56 synthesized Ca–Zn/ZSM-5 by the consecutive impregnation method, varying the Ca loading on the Zn/ZSM-5 catalyst. They report that adding 0.02 % wt. Ca can recover the Brønsted acid site (BAS) acidity, which decreases with Zn, and simultaneously improve the selectivity for aromatic compounds and BTX. Researchers synthesized micropore Ni/Zn/ZSM-5 using the co-impregnation method. It was demonstrated that Ni can stabilize Zn, reduce Zn loss during the process, and minimize coke formation, thereby extending catalyst lifetime.10 Wang et al.4 reported that Ce addition to Zn/ZSM-5 improved co-aromatization performance with n-hexane co-feeding, and a related study58 found that Ce-modified hierarchical Zn/ZSM-5 enhanced aromatic stability. The relevance of Zn incorporation method (hydrothermal substitution vs. post-synthetic impregnation) to MTA performance has been directly demonstrated,59 reinforcing the one-pot in situ strategy adopted here. Dry-gel-conversion routes combining Zn and P have produced hierarchical Zn–P/ZSM-5 with improved BTX stability,60 and orientation-controlled ZSM-5 growth has been shown to influence selectivity independently of metal promotion.47 Furthermore, Xin and co-workers61 introduced a bimetallic Zn–Sn/HZSM-5 catalyst, achieving a BTX yield of 64.1% by adding Sn as a second promoter to the Zn/ZSM-5 catalyst; however, this approach caused faster deactivation of micropore ZSM-5. In another study, ZSM-5 zeolite combined with specific zinc and phosphorus species achieved excellent selectivity (85%) for BTX among the aromatic products. These species create strong Lewis acid centers and an optimized surface acidity distribution, favoring BTX formation and improving the catalyst's hydrothermal stability.62

Ni and Cr were deliberately selected as a contrasting pair of secondary promoters based on their distinct redox chemistry and coordination behavior with Zn, rather than as arbitrarily interchangeable dopants. Ni2+ readily undergoes partial reduction to Ni0/Ni-delta+ under the reaction/calcination conditions used here, enabling hydrogen overflow and electronic interaction with adjacent Zn sites, which is expected to stabilize hydroxylated, catalytically active Zn(OH)+ and the Brønsted framework with moderate acid strength. Cr predominantly adopts stable Cr3+ (and some Cr6+) states that resist reduction and tend to form separate CrOx/Cr2O3 domains or Zn–Cr spinel (ZnCr2O4), reducing its capacity to stabilize Zn(OH)+ and instead introducing additional strong Lewis's acidity. Selecting two metals of opposing redox accessibility and Zn-stabilizing capacity allows the resulting differences in Zn speciation, acid-site balance, and coke resistance (Sections 3.1.5, 3.1.6, 3.2.5) to be attributed to a specific, identifiable mechanistic contrast rather than to generic metal doping effects. Both Ni5,63 and Cr64,65 are independently reported to enhance aromatic selectivity; because of this contrasting mechanistic potential, they are used as promoters in this work. These studies, together with recent progress reviews on deactivation resistance in Zn-ZSM-5,66 motivate the systematic comparison of Zn–Ni and Zn–Cr undertaken here.

In a previous related study, the effects of water-soluble polymer secondary templates (PVP and PEG) on the textural and acid properties of unmodified hierarchical ZSM-5 for MTA were investigated, and PVP was identified as a more effective template for balanced micro-mesoporosity.58 That study did not include a dehydrogenation-active metal and therefore could not address metal speciation, Zn(OH)+ formation, or bimetallic synergism. Three questions remain unanswered in the broader literature: (i) how Zn can be directly incorporated into PVP-assisted one-pot synthesis and how this affects Zn dispersion/speciation; (ii) how a second transition-metal promoter (Ni or Cr) modifies this speciation and the resulting acid-site balance within a hierarchical, PVP-templated framework, as opposed to conventional microporous or desilicated supports used in most bimetallic Zn-promoter studies;10,21,55–57 and (iii) how these metal-base interactions translate into time stability in flow and coke deposition pathways. The present work addresses this three-part gap by systematically comparing Zn@ZC, Zn@DS/ZC, Zn@PVP/ZC, ZnCr@PVP/ZC, and ZnNi@PVP/ZC, with particular focus on linking XPS-quantified Zn(OH)+ abundance to BTX selectivity and deactivation resistance.

2. Experimental section

2.1. Materials

The experiment involved the use of various reagents, including tetraethyl orthosilicate (TEOS), sodium aluminate (NaAlO2), sodium hydroxide (NaOH), n-butyl amine (NBA), polyethylene glycol with a molecular weight of 10 000 (PEG), zinc nitrate hexahydrate, chromium(iii) nitrate nonahydrate, and nickel(ii) nitrate hexahydrate, all obtained from Merck. Furthermore, polyvinylpyrrolidone K12 with a molecular weight of 3500 (PVP) was acquired from Thermo Scientific Chemicals, and methanol was sourced from Dr Mojallali Industrial Chemical Complex Co. All reagents were utilized without any prior purification.

2.2. Catalyst preparation

2.2.1. Convectional microporous Zn@ZSM-5 synthesis

The conventional Zn-containing ZSM-5 catalyst, denoted as Zn@ZC, was synthesized through a hydrothermal procedure. Initially, NaAlO2 (0.21 g) and NaOH (0.26 g) were dissolved in 48 mL of deionized water and stirred for 30 min at ambient temperature. After complete dissolution, 2.43 g of n-butylamine (NBA) was introduced as the structure-directing agent. Subsequently, 13.8 g of tetraethyl orthosilicate (TEOS) was slowly added under continuous stirring, and the resulting mixture was maintained under agitation for 90 min until a homogeneous precursor gel was obtained. Thereafter, Zn(NO3)2·6H2O was incorporated into the synthesis mixture in an amount corresponding to 1 wt% Zn in the final catalyst. The suspension was further stirred for 1 h to ensure uniform distribution of the zinc species. The resulting synthesis gel possessed a molar composition of Si: 0.02 Al2O3: 0.5 NBA: 0.1 NaOH: 40H2O: 0.011 Zn.

The prepared gel was transferred into a Teflon-lined stainless-steel autoclave and subjected to hydrothermal crystallization at 180 °C for 48 h. Following crystallization, the solid product was recovered by filtration, thoroughly washed with deionized water until a neutral pH was reached, dried overnight at 110 °C, and finally calcined in air at 550 °C for 5 h.

2.2.2. Hierarchical desilicated ZSM-5 synthesis

Hierarchical Zn@DS/ZC was obtained via post-synthetic alkaline treatment of the parent Zn@ZC sample. In a typical experiment, 5 g of Zn@ZC was dispersed in 0.2 M NaOH solution using a liquid-to-solid ratio of 30 : 1. The suspension was maintained at 70 °C for 60 min under stirring to selectively remove framework silicon and generate mesoporosity.

After treatment, the catalyst was separated from the alkaline medium by filtration, repeatedly washed with distilled water, and dried overnight at 110 °C. The dried material was subsequently calcined at 550 °C for 5 h to obtain the final desilicated catalyst.

2.2.3. One-pot Hierarchical Zn@ZSM-5 synthesis

A one-pot hydrothermal route was employed to prepare hierarchical Zn-containing ZSM-5 using PVP as a secondary mesostructure-directing agent. First, NaAlO2 and NaOH were dissolved in deionized water, followed by the addition of NBA under continuous stirring. PVP was then introduced into the solution and allowed to interact with the precursor mixture for 30 min prior to silica addition.

Subsequently, TEOS was slowly introduced into the reaction medium. After gel formation, Zn(NO3)2·6H2O was added to provide a zinc loading of 1 wt% in the final catalyst. The mixture was further stirred for 1 h to ensure homogeneous incorporation of zinc species within the synthesis gel. The molar composition of the synthesis mixture was Si: 0.02 Al2O3: 0.5 NBA: 0.2 Na: 60H2O: 0.0066 PVP: 0.011 Zn.

The precursor gel was transferred to an autoclave and crystallized at 180 °C for 48 h. The resulting solid was collected by filtration, washed repeatedly with deionized water until neutral pH, dried overnight at 110 °C, and calcined at 550 °C for 5 h. The resulting hierarchical Zn-modified catalyst is hereinafter designated as Zn@PVP/ZC.

2.2.4. One-pot hierarchical dual promoter Zn@ZSM-5 synthesis

Bimetallic hierarchical catalysts containing Zn together with either Ni or Cr were prepared following the same hydrothermal procedure used for Zn@PVP/ZC. During gel preparation, the required amount of Ni(NO3)2·6H2O or Cr(NO3)3·9H2O was simultaneously introduced with the zinc precursor, allowing co-incorporation of both metal species during crystallization. The resulting samples were designated as ZnNi@PVP/ZC and ZnCr@PVP/ZC, respectively.

To convert all synthesized catalysts into their protonic form, ion-exchange treatment was carried out using a 1 M NH4NO3 solution with a solution-to-solid ratio of 20 : 1. The exchange process was performed at 80 °C for 3 h and repeated twice. Finally, the exchanged samples were dried overnight at 110 °C and calcined at 550 °C for 5 h to obtain the H-form catalysts.

2.3. Catalyst characterization

The structural properties and phase purity of the prepared zeolite samples were evaluated by powder X-ray diffraction (XRD) using a Philips X'Pert Pro diffractometer operating with Cu Kα radiation (λ = 1.544 Å). Diffraction data were collected over a 2θ interval of 5–50°. Relative crystallinity was measured using the integrated peak-area method (2θ = 22–25°), in accordance with ASTM D5758 standards for ZSM-5. This method typically has a measurement uncertainty of only a few percentage points.

Infrared spectroscopy was employed to investigate the framework vibrations and surface functional groups of the catalysts. FTIR spectra were recorded in the wavenumber range of 400–4000 cm−1 using a PerkinElmer Spectrum 65 instrument. Prior to analysis, each sample was finely mixed with KBr and compressed into pellets.

The textural characteristics of the zeolites were determined from nitrogen adsorption–desorption measurements carried out on a BELSORP Mini II analyzer. Before measurement, the samples were evacuated at 200 °C under vacuum for 3 h to remove adsorbed species. Specific surface areas were derived using the Brunauer–Emmett–Teller (BET) equation, whereas pore size distributions were obtained from the desorption branch through the Barrett–Joyner–Halenda (BJH) method. The total pore volume was estimated at a relative pressure (P/P0) of 0.99, while micropore parameters were calculated using the t-plot model. Each sample was analyzed by at least two replicate N2 physisorption measurements, and the BET surface area and pore-volume values reported in Table 1 represent the average of these replicates.

Table 1. Physico-chemical properties of the prepared catalysts.

Catalyst R.C. (%)a S BET (m2 g−1)b S micro (m2 g−1)c S ext (m2 g−1)d V total (cm3 g−1)e V micro (cm3 g−1)f V meso (cm3 g−1)g
Zn@ZC 100 300.2 250.4 49.8 0.173 0.161 0.012
Zn@DS/ZC 72.3 342.4 255.9 86.5 0.304 0.100 0.204
Zn@PVP/ZC 91.2 333.1 257.0 76.1 0.276 0.097 0.179
ZnCr@PVP/ZC 93.2 309.8 240.3 69.5 0.246 0.088 0.158
ZnNi@PVP/ZC 97.6 323.9 253.5 70.4 0.248 0.087 0.161
a

Relative crystallinity by XRD data.

b

Obtained by the BET method using adsorption data.

c

Measured by t-plot method.

d

S ext = SBET − Smicro.

e

Estimated from the adsorbed amount at p/p0 = 0.99.

f

Measured by t-plot method.

g

V meso = Vtotal − Vmicro.

The chemical composition of the synthesized materials, particularly the Si and Al contents, was quantified by inductively coupled plasma optical emission spectroscopy (ICP-OES) using a Spectro Arcos analyzer.

The morphologies of the samples were examined using scanning electron microscopy (SEM). SEM analysis was performed with a TESCAN MIRA-3 SEM operating at 20 kV. Before imaging, samples were coated with a 15–20 nm gold layer using Q150 R ES by Quorum Co. X-ray photoelectron spectroscopy (XPS) experiments were performed using a BESTEC EA10 spectrometer system with a monochromatic Al Kα (1486.6 eV) X-ray source. The binding energy (BE) values were calibrated using the C 1s peak at 284.9 eV.

The acidity of the sites was assessed by temperature-programmed desorption (TPD) of ammonia using a NanoSORD Sensiran Co. instrument. Catalyst samples were first cleaned by flowing N2 at 300 °C for 1 hour, then cooled to 100 °C. Subsequently, they were exposed to an atmosphere containing 10% NH3 in He for 1 hour to saturate with ammonia. TPD measurements were carried out from 100 to 700 °C at a heating rate of 10 °C min−1. Total acid-site density was determined from the NH3-TPD profile as follows: the total NH3 uptake during the saturation step (10% NH3/He, 100 °C, 1 h) was first quantified from the TCD signal using a calibration curve constructed from known NH3 pulse volumes, giving the total ammonia uptake per gram of catalyst (mmol NH3/g). This total uptake was then used as the calibration reference for the subsequent TPD desorption profile: after linear baseline correction, the total integrated area under the TPD curve (100–700 °C) was set equal to this total NH3 uptake, and the area of each of the two deconvoluted Gaussian components (Section 3.1.6) was converted to an absolute ammonia-desorption quantity (mmol g−1) in direct proportion to its fractional share of the total integrated area. Weak- and strong-acid-site densities (Table 3) thus represent the fraction of total NH3 uptake desorbing below ∼300 °C and above ∼350–450 °C, respectively, and their sum equals the independently measured total acidity.

Table 3. Acidic properties of catalysts.

Catalyst Weak acidity (mmol g−1) Strong acidity (mmol g−1) Total acidity (mmol g−1)
Zn@ZC 0.393 0.299 0.692
Zn@DS/ZC 0.431 0.285 0.716
Zn@PVP/ZC 0.455 0.490 0.944
ZnCr@PVP/ZC 0.274 0.428 0.702
ZnNi@PVP/ZC 0.563 0.381 0.944

Thermogravimetric analysis (TGA) of the catalysts after the MTA reaction was performed using a Netzsch TGA 209 F1. The analysis was carried out at a 10 °C min−1 ramp in an air atmosphere, reaching 900 °C, to investigate coke formation on the catalysts.

The apparent activation energy (Ea) and pre-exponential factor (A) for coke combustion were determined from the TGA weight-loss profiles using the Coats–Redfern method.85 The fractional conversion at each temperature was defined as α = (mo − mt)/(mo − m∞), where mo, mt, and m∞ are the initial, instantaneous, and final sample mass, respectively. Assuming first-order combustion kinetics, the Coats–Redfern linearization gives ln[−ln(1 − α)/T2] vs. 1/T a straight line over the conversion range α = 0.1–0.9, with slope = −Ea/R and intercept related to A (min−1), the pre-exponential factor of the Arrhenius rate expression, via A = exp(intercept)·(βEa/R), where β is the heating rate (10 °C min−1), and R is the universal gas constant. Ea and A were obtained by linear regression of this plot for each catalyst (Table 5). Also, the relative contribution of internal coke was estimated from the loss in micropore volume between the fresh and spent catalysts, following the approach of ref. 68: internal coke mass (mg g−1 catalyst) = (Vmicro-fresh − Vmicro-spent) [cm3 g−1] × 1.22 [g cm−3] × 1000. The internal coke fraction (%) reported in Table 5 was calculated as the ratio of this internal coke mass to the total coke mass determined by TGA, with the external coke fraction obtained by difference (100% − internal coke %).

Table 5. Coke analysis dataa.

Catalyst Coke amount (mg) Coke rate g coke g−1catalyst min−1 Internal coke (%)a External coke (%) A (min−1) E a (kJ mol−1)
Zn@ZC 115.8 6.44 × 10−5 82.6 17.4 0.611 23.2
Zn@DS/ZC 89.8 4.99 × 10−5 65.5 34.5 0.707 24.2
Zn@PVP/ZC 73.3 4.07 × 10−5 59.4 40.6 13.2 34.9
ZnCr@PVP/ZC 77.2 4.29 × 10−5 66.2 33.8 1.62 25.6
ZnNi@PVP/ZC 40.0 2.22 × 10−5 46.7 53.3 0.952 23.8
a

Internal coke has been calculated based on Zhou et al.68

2.4. Catalytic performance test

Catalytic testing for methanol aromatization was carried out in a stainless-steel fixed-bed reactor (10 mm i.d., 100 cm length) operated under continuous-flow conditions as shown in Fig. 1. For each experiment, 0.6 g of catalyst particles (20–40 mesh) was diluted with 1.8 g of inert sea sand (10–20 mesh) to improve heat distribution within the catalyst bed.

Fig. 1. Schematic representation of experimental setup.

Fig. 1

Prior to reaction, the catalyst was activated under a nitrogen atmosphere at 450 °C for 1.5 h using a gas flow rate of 40 mL min−1. After activation, the reactor temperature was adjusted to the reaction temperature of 400 °C and maintained throughout the experiment. The temperature inside the catalyst bed was continuously monitored using a K-type thermocouple positioned at the center of the reactor.

Methanol was continuously fed into the reactor by means of a syringe pump at a weight hourly space velocity (WHSV) of 5 h−1. Nitrogen was simultaneously introduced as the carrier gas at 40 mL min−1. The reactor effluent was passed through a water-cooled condenser, allowing separation of condensable products from the gaseous fraction.

Product analysis was performed using a Varian Star 3800 gas chromatograph equipped with flame ionization (FID) and thermal conductivity (TCD) detectors. The condensed liquid phase and gaseous products were quantified to determine methanol conversion, product selectivities, and carbon-based space-time yield according to the equations (eqn (1) and eqn (2)) presented below:

2.4. 1
2.4. 2
Carbon-based space-time yield = WHSV × conversion × selectivity (gC. gcat−1 h−1) 3

where A represents the peak area, and n represents the number of carbon atoms in the product i.

To ensure reproducibility, each catalytic test was performed at least three times under identical conditions, and the variations in methanol conversion and product selectivity were within +/−2%. The carbon balance ranged from 97% to 102% across all catalytic runs, consistent with acceptable closure for fixed-bed MTA systems.

3. Results and discussion

3.1. Catalysts characterization

3.1.1. XRD analysis

The crystallographic characteristics of the prepared catalysts were examined by XRD, and the resulting patterns are presented in Fig. 2.

Fig. 2. XRD spectra of the prepared ZSM-5 catalysts.

Fig. 2

Regardless of the synthesis route or metal composition, all samples exhibit diffraction signatures consistent with the ZSM-5 MFI topology. The observed reflections at approximately 8.0°, 8.8°, 23.1°, 23.9°, and 24.3° can be attributed to the (101), (200), (501), (151), and (303) crystal planes, demonstrating that the zeolite framework was successfully developed and retained after modification.20,41,50 The relative crystallinity of the samples was quantified from the peak area within the 2θ range of 22–25°, using the crystalline Zn@ZC sample as a reference (Table 1). Furthermore, the absence of diffraction peaks associated with metal species in the metal-loaded ZSM-5 patterns suggests that the metals are either highly dispersed or present as ultrafine particles within the zeolite matrix.

The relative crystallinity of Zn@DS/ZC is approximately 72.3%, compared to 100% for the reference Zn@ZC sample. This decrease can be attributed to the alkali treatment, which introduces defects into the zeolitic framework and consequently lowers crystallinity.29,30 In contrast, Zn@PVP/ZC exhibits a higher relative crystallinity of 91.2%, indicating that the presence of PVP may facilitate69 the nucleation and growth of ZSM-5 crystals. However, due to the steric hindrance of PVP chains, its crystallinity remains slightly lower than that of the untreated reference. Notably, samples containing dual metal promoters exhibit even higher crystallinity, a trend that runs counter to the common expectation that metal incorporation reduces crystallinity; the distinct mechanisms responsible for Ni and Cr are discussed below. While Zn incorporation alone tends to reduce crystallinity due to formation of ZnO, the addition of Ni or Cr enhances the interaction between the metals and the zeolite framework, albeit through distinct mechanisms. XPS quantification (Section 3.1.5, Table 2) shows that Ni incorporation markedly suppresses bulk ZnO formation, decreasing the ZnO fraction from 32.8% in Zn@PVP/ZC to 12.6% in ZnNi@PVP/ZC while correspondingly increasing catalytically active Zn(OH)+ species to 87.4%, consistent with its higher relative crystallinity (97.6%, Table 1). In contrast, Cr incorporation does not suppress ZnO formation—instead, the ZnO fraction increases slightly to 40.1% in ZnCr@PVP/ZC—and its improved crystallinity relative to Zn@ZC is more likely attributable to its lower overall Al rather than Zn dispersion effects. Lower Al incorporation is generally associated with reduced framework strain and fewer Al-related defect sites during hydrothermal crystallization,70 consistent with the preserved crystallinity observed here despite the absence of ZnO suppression.

Table 2. Elemental analysis data.
Catalyst Si/Ala Si/Alb Zn (%)c Cr (%)c Ni (%)c Zn state distribution (%)
ZnO Zn(OH)+
Zn@ZC 25.1 13.6 0.73 — — 73.9 26.1
Zn@DS/ZC 23.9 14.3 0.7 — — 70.6 29.4
Zn@PVP/ZC 20.3 16.1 0.86 — — 32.8 67.2
ZnCr@PVP/ZC 22.6 18.3 0.82 0.91 — 40.1 59.9
ZnNi@PVP/ZC 20.5 15.4 0.93 — 0.92 12.6 87.4
a

Bulk Si/Al ratio by ICP.

b

Surface Si/Al ratio by XPS.

c

Metal wt% by ICP.

Notably, relative crystallinity alone does not linearly track BTX selectivity across the catalyst series (Table 4). Zn@ZC has the highest crystallinity but the lowest BTX selectivity (32.4%), reflecting its purely microporous, diffusion-limited architecture (Section 3.1.3). In contrast, ZnCr@PVP/ZC is more crystalline than Zn@PVP/ZC (93.2% vs. 91.2%) but has lower BTX selectivity (50.4% vs. 61.8%), consistent with its stronger acid-site density (Section 3.1.6) outweighing the structural advantage. Relative crystallinity is therefore a necessary but insufficient structural descriptor; its catalytic significance must be assessed alongside mesoporosity and acid-site/Zn-speciation.

Table 4. Product selectivity for MTA reaction over the ZSM-5 samplesa.
Catalyst Selectivity (%) BTX selectivity (%) STY (gC gcat−1 h−1)
C1 C2–C4 C2–C4 Created by potrace 1.16, written by Peter Selinger 2001-2019 C5+ Aromatic B T X BTX C9+ BTX Aromatic
Zn@ZC 1.8 38.0 10.5 10.2 39.5 8.3 12.9 11.2 32.4 7.1 1.61 1.97
Zn@DS/ZC 1.7 26.4 13.2 7.0 51.7 8.9 15.7 14.3 38.9 12.8 1.94 2.57
Zn@PVP/ZC 2.1 15.5 9.6 5.5 67.3 7.1 21.5 33.2 61.8 5.5 3.07 3.35
ZnCr@PVP/ZC 2.9 22.8 4.5 8.7 61.1 6.2 18.5 25.7 50.4 10.7 2.51 3.04
ZnNi@PVP/ZC 2.5 15.3 5.9 4.5 71.8 7 16.5 44.4 67.9 3.9 3.38 3.57
a

Reaction conditions: TOS = 3 h, atmospheric pressure, 0.6 g catalyst, 400 °C, WHSV = 5 h−1. The methanol conversion is 99.5% across all samples. C1: methane, C2–C4 alkanes hydrocarbons, C2–C4 = olefin hydrocarbons, C5+ aliphatic hydrocarbons, B: benzene, T: toluene, X: xylenes, C9+: heavy C9+ aromatic hydrocarbon.

3.1.2. FT-IR analysis

Fig. 3 displays the infrared spectra of the prepared zeolitic materials. Independent of the synthesis route, all samples exhibit spectral features consistent with the MFI topology, confirming preservation of the ZSM-5 framework.

Fig. 3. (a) FT-IR spectrum of ZSM-5 adsorbents in the range of 400–2600 cm−1, (b) FT-IR spectrum of ZSM-5 adsorbents in the range of 2600–4000 cm−1.

Fig. 3

The low-wavenumber bands at about 450–470 cm−1 and 550–560 cm−1 are related to framework deformation vibrations and the characteristic double five-membered ring structure, respectively. Meanwhile, the absorptions detected in the regions of 790–800, 1050–1100, and 1220–1230 cm−1 originate from different stretching modes of Si–O–Si and Si–O–Al linkages within the zeolite lattice.71,72 Peak-position analysis shows that the T–O–T symmetric and asymmetric stretching bands (796.4 and 1035.5 cm−1) and the H–O–H bending mode of physisorbed water (1629.5 cm−1) are consistent across all five catalysts. This suggests that the main Si–O–Si/Si–O–Al connectivity remains unchanged with metal addition. Conversely, the low-frequency framework deformation band shifts from 453.1 cm−1 in Zn@ZC to 447.4 cm−1 in Zn@DS/ZC (a 5.7 cm−1 redshift), and to 458.9 cm−1 in Zn@PVP/ZC (a 5.8 cm−1 blueshift). Adding a second promoter shifts this band to 451.0 cm−1 (ZnCr@PVP/ZC) and 454.0 cm−1 (ZnNi@PVP/ZC). The double five-membered-ring vibration shifts from 545.0 cm−1 (Zn@DS/ZC) to 547.0 cm−1 (Zn@PVP/ZC and ZnCr@PVP/ZC) and 549.0 cm−1 (ZnNi@PVP/ZC). These shifts may be attributed to metal incorporation into the zeolite channels and interactions with the ZSM-5 framework.73,74

Furthermore, the broad band observed near 3451 cm−1 indicates the presence of hydroxyl-rich defect sites, typically associated with interconnected silanol groups linked through hydrogen-bond interactions. The distinct band observed at 3610 cm−1 corresponds to Brønsted acidic Si–OH–Al groups, confirming the presence of bridging hydroxyl species associated with framework aluminum. In addition, the band near 3665 cm−1 is assigned to extra-framework or partially hydrolyzed aluminum species, while the absorption at 3740 cm−1 is attributed to isolated external silanol groups on the zeolite surface. Moreover, the weak feature observed around 3720 cm−1 is associated with free internal silanol groups within the zeolitic channels.

Observed variations in the hydroxyl-region bands indicate changes in acidic environment of the catalyst. In ZSM-5-based materials, the framework hydroxyl groups are closely associated with Brønsted acid sites which are responsible for methanol activation and hydrocarbon pool intermediate formation. Therefore, changes in hydroxyl-band intensity suggest modifications in acid-site distribution resulting from polymer-assisted synthesis and promoter incorporation.

The FT-IR observations are consistent with the NH3-TPD and XPS results. In particular, Ni promotion favored the formation of Zn(OH)+ species, increased the relative contribution of weaker acid sites, and moderated the concentration of strong acid sites. This balance facilitates aromatization and BTX formation while suppressing excessive hydrogen-transfer reactions, coke formation, and catalyst deactivation. Consequently, the catalyst with the most favorable hydroxyl-site characteristics also exhibited the highest BTX selectivity and the lowest coke deposition.

3.1.3. N2- adsorption–desorption analysis

To investigate the pore structure of the catalysts, N2 adsorption–desorption measurements were performed, and the results are presented in Fig. 4a and Table 1.

Fig. 4. (a) N2 adsorption–desorption isotherms, (b) BJH pore size distribution plot.

Fig. 4

The isotherm of Zn@ZC exhibits a typical type-I pattern, characterized by a steep adsorption occurring at low relative pressure levels (P/P0 < 0.1) followed by a plateau extending to higher pressures (0.4 < P/P0 < 0.9). This observation indicates that the parent ZC zeolite mainly exhibits microporous characteristics with only a small degree of mesoporosity.9

In contrast, the samples Zn@DS/ZC, Zn@PVP/ZC, ZnCr@PVP/ZC, and ZnNi@PVP/ZC display type-IV isotherms with an H4-type hysteresis loop in the range of P/P0 = 0.4–0.99, indicating the coexistence of micropores and mesopores.45,50

The textural parameters derived from these measurements are summarized in Table 1. The Zn@ZC sample exhibits a specific surface area of 300.2 m2 g−1 and a total pore volume of 0.173 cm3 g−1. After alkali treatment, the Zn@DS/ZC sample shows a remarkable increase in surface area and total pore volume, reaching 342.4 m2 g−1 and 0.304 cm3 g−1, respectively. This enhancement is mainly due to the generation of mesopores through partial desilication, as evidenced by the increase in Sext (from 49.8 to 86.5 m2 g−1) and Vmeso (from 0.012 to 0.204 cm3 g−1).

Similarly, the Zn@PVP/ZC catalyst exhibits a high surface area (333.1 m2 g−1) and total pore volume (0.276 cm3 g−1). The mesopore and micropore volumes are 0.179 cm3 g−1 and 0.097 cm3 g−1, respectively, suggesting that the addition of PVP successfully generates a hierarchical mesoporous structure while maintaining the intrinsic microporosity and crystallinity of the zeolite. The incorporation of a second metal promoter (Ni or Cr) slightly reduces the surface area and total pore volume compared to Zn@PVP/ZC, likely due to partial pore blockage or metal deposition on the zeolite surface. The specific surface areas and total pore volumes are 309.8 m2 g−1 and 0.246 cm3 g−1 for ZnCr@PVP/ZC, and 323.9 m2 g−1 and 0.248 cm3 g−1 for ZnNi@PVP/ZC, respectively.

The reduction in BET surface area and pore volume after the addition of promoter is probably due to the partial filling of accessible pores by Ni- and Cr-containing species. This behavior aligns with reports on metal-modified ZSM-5 catalysts, in which metal species partially cover internal and external surfaces, decreasing the measured surface area. Furthermore, SEM images didi not show any significant particle agglomeration, indicating that the decrease in surface area is more probably due to pore occupation rather than particle growth.

The BJH pore size distribution illustrated in Fig. 3b shows that the Zn@ZC sample features the largest portion in the microporous area, indicating a significant presence of pores measuring approximately 1–2 nm in diameter. The Zn@DS/ZC sample demonstrates a larger contribution within the mesopore area, particularly in the 3–6 nm range. The PVP-modified samples are identified by mesopores primarily found within the 2–6 nm range, alongside some contribution in the 10–20 nm range.

The hierarchy between these pore regimes is directly relevant to BTX transport: the native ZSM-5 micropore channels (5.1–5.6 Å) are comparable to or smaller than the molecular dimensions of BTX species intersection diameter of ZSM-5 (ref. 25)—whereas the mesopores generated here (2–20 nm) are one to two orders of magnitude larger and present no comparable restriction. This size contrast provides a structural basis for the coke-distribution trends discussed in Section 3.2.5, where increasing mesoporosity systematically shifts coke deposition from internal (micropore-confined) to external surfaces, consistent with easier outward diffusion of bulky aromatic intermediates before secondary hydrogen-transfer and condensation reactions can occur.

To evaluate the extent of hierarchical mesoporosity as shown by the BJH profiles, the mesopore volume fraction (Vmeso/Vtotal from Table 1) was compared among the catalysts. Zn@ZC exhibits a mesopore fraction of just 6.9% (Vmicro/Vtotal = 93.1%), confirming its predominantly microporous. Alkaline desilication increases this to 67.1% in Zn@DS/ZC, while the PVP-templated samples display similarly high mesopore fractions of 64.9% (Zn@PVP/ZC), 64.2% (ZnCr@PVP/ZC), and 64.9% (ZnNi@PVP/ZC). Although the overall bulk mesopore fraction is nearly the same, the external-to-total surface area ratio (Sext/SBET) decreases slightly from 25.3% (Zn@DS/ZC) to 22.8% (Zn@PVP/ZC), 22.4% (ZnCr@PVP/ZC), and 21.7% (ZnNi@PVP/ZC). This suggests that PVP treatment favors the formation of more intracrystalline (shape-selective) mesoporosity over external, defect-related porosity, consistent with the higher relative crystallinity observed in the PVP-templated samples (Table 1).

Overall, these results confirm that using secondary templates and metal promoters effectively adjusts the hierarchical textural properties of ZSM-5, striking a balance between mesoporosity creation and framework preservation.

3.1.4. Morphology analysis by SEM

SEM analysis provides insight into the morphological features of the synthesized ZSM-5-based catalysts. As illustrated in Fig. 5a, the parent Zn@ZC zeolite exhibits an agglomerated intergrown flower-like morphology with an average particle size of approximately 16.3 µm.

Fig. 5. SEM images of (a) Zn@ZC, (b) Zn@DS/ZC, (c) Zn@PVP/ZC.

Fig. 5

In addition, particle size distributions were obtained by manually measuring approximately 100–120 individual particles per sample across multiple SEM micrographs at different fields of view to ensure statistically representative sampling.

After desilication, the Zn@DS/ZC sample (Fig. 4b) develops a more defined coffin-shaped morphology, accompanied by a slight increase in crystal size to around 20.2 µm.

Upon introducing PVP as a secondary template, the morphology of Zn@PVP/ZC (Fig. 4c) transforms into a multilamellar, coffin-like hexagonal structure. This transformation is attributed to the dual hydrophilic and hydrophobic nature of PVP, which enables it to interact with both amorphous precursors and the zeolitic framework, thereby modulating nucleation and crystal growth. Specifically, the pyrrolidone units in PVP, through their lactam carbonyl (–C Created by potrace 1.16, written by Peter Selinger 2001-2019 O) and tertiary amine groups, can form hydrogen bonds or coordination interactions with Al–OH and Si–OH groups on the surfaces of developing nuclei.38 Such interactions, coupled with the steric hindrance of polymer chains, effectively restrict crystal growth, particularly along the b-axis, leading to the formation of thinner, sheet-like crystals with reduced particle size (∼6.7 µm). The influence of secondary metal promoters on morphology is further illustrated in Fig. 6a and b.

Fig. 6. SEM images of (a) ZnCr@PVP/ZC, (b) ZnNi@PVP/ZC.

Fig. 6

The ZnCr@PVP/ZC sample exhibits fragmented prismatic crystals with an average particle size of approximately 4.5 µm. In contrast to the thin, stacked plates observed in Zn@PVP/ZC, this sample exhibits a smoother, more compact surface, indicating that Cr incorporation alters the crystal growth pattern during crystallization. In contrast, the ZnNi@PVP/ZC sample maintains a multilamellar hexagonal or rectangular crystal morphology similar to Zn@PVP/ZC, though with greater irregularity and a smaller mean size of about 2.37 µm. This reduction in particle size can be attributed to the incorporation of secondary promoters, as Zhang Y et al.64 describe the atomic radii of Cr (128 pm), Ni (124 pm), and Al (143 pm) facilitate enhanced nucleation and accelerated crystal growth, ultimately yielding smaller, more compact zeolite particles.

3.1.5. Elemental analysis by XPS and ICP

Elemental characterization of the synthesized materials was performed using XPS and ICP techniques. The combination of these two analytical methods enables a detailed assessment of both surface and bulk compositions, providing essential evidence for the successful incorporation of metal species into the zeolite framework. As shown in Table 2, the bulk Si/Al ratio for the microporous Zn@ZC sample is 25.1. After the desilication treatment, as expected, the Si/Al ratio decreases to 23.9 due to the removal of Si from the zeolite framework. According to the literature, Zn can stabilize Al during desilication and provide uniform desilication.75

PVP template samples (Zn@PVP/ZC, ZnCr@PVP/ZC, and ZnNi@PVP/ZC) showed a lower Si/Al ratio, which indicates that PVP introduces more Al into the zeolite framework. Zn percentage is also measured by ICP analysis. Zn@ZC shows 0.73% Zn by weight. In many ZSM-5 syntheses, in situ incorporation of transition metals yields significantly lower metal loadings than post-synthesis impregnation.

The relatively low metal loading observed in the samples can be attributed to the zeolite framework's limited capacity to incorporate metal ions during hydrothermal synthesis. Only a fraction of the metal species can be stabilized within the structure, while excess species may remain in the synthesis medium or form non-framework clusters. The slight decrease in Zn content after desilication (from 0.73 to 0.70 wt%) is associated with partial leaching of zinc species during the alkaline treatment used to generate mesopores.

The presence of PVP significantly enhances Zn incorporation, resulting in a higher Zn content (up to 0.86 wt%) in Zn@PVP/ZC compared with the conventional microporous Zn@ZSM-5 catalyst. This behavior is attributed to the stabilizing and dispersion-promoting role of PVP69,71 during synthesis, which facilitates more effective metal retention within the zeolite structure.

In the PVP-assisted bimetallic samples, the Zn loading depends on the nature of the second metal. ZnNi@PVP/ZC exhibits higher Zn content than ZnCr@PVP/ZC, likely due to stronger synergistic interactions between Ni and Zn species that improve Zn stabilization and dispersion. In contrast, the relatively lower Zn content in ZnCr@PVP/ZC may be related to competitive incorporation effects or the formation of chromium oxide species that partially limit Zn inclusion within the zeolite framework.

These Si/Al trends correlate directly and consistently with the acid-site densities measured by NH3-TPD (Table 3). Among the three PVP-templated samples, the surface Si/Al ratio (XPS) shows a clean inverse relationship with weak acid-site density: ZnNi@PVP/ZC exhibits both the lowest surface Si/Al ratio (15.4) and the highest weak acidity (0.563 mmol g−1); Zn@PVP/ZC is intermediate (16.1; 0.455 mmol g−1); ZnCr@PVP/ZC shows the highest surface Si/Al ratio (18.3) alongside the lowest weak acidity (0.274 mmol g−1). A complementary relationship links the bulk Si/Al ratio (ICP) to total acidity: Zn@PVP/ZC and ZnNi@PVP/ZC share the lowest bulk ratios (20.3, 20.5) and highest total acidity (0.944 mmol g−1 for both), whereas ZnCr@PVP/ZC, with the highest bulk ratio (22.6), shows the lowest total acidity (0.702 mmol g−1). The bulk Si/Al ratio thus sets an upper bound on total acid-site density, while the surface Si/Al ratio, as modulated by the specific secondary metal, governs how this acidity is partitioned between weak and strong sites.

Table 2 summarizes the XPS results for the surface Si/Al ratios of the synthesized catalysts. The parent Zn@ZC sample exhibits a Si/Al ratio of 13.6, consistent with the characteristic composition of conventional ZSM-5. Upon desilication, partial removal of extra-framework aluminum slightly increases this ratio to 14.3, indicating the partial dealumination of the zeolitic surface. In contrast, the introduction of PVP during one-pot synthesis enhances the effective incorporation of aluminum into the zeolite framework. PVP likely directs Al species into tetrahedral framework sites while reducing the amount of extra-framework Al on the surface, resulting in an increased Si/Al ratio of 16.1 for the Zn@PVP/ZC sample.

Further modification with secondary metal promoters has a significant impact on the surface composition. The Cr-containing sample (ZnCr@PVP/ZC) shows the highest Si/Al ratio (18.3), suggesting that this may be associated with modifications in the surface distribution of aluminum species induced by the presence of Cr during synthesis. Conversely, Ni incorporation leads to a Si/Al ratio of 15.4, suggesting that Ni primarily interacts with framework Al, possibly through partial isomorphic substitution or stable coordination, thereby helping retain more surface-accessible Al than Cr.

Overall, these observations indicate that PVP-assisted synthesis influences Al speciation by promoting deeper framework incorporation, while the type of secondary metal (Ni or Cr) determines whether Al remains framework-bound and accessible or becomes redistributed and partially masked. This interplay directly affects the acidity distribution and, consequently, the catalytic performance of the materials.

The state of surface Zn species across different samples was further examined using Zn (2p3/2) XPS spectra. As shown in Fig. 7a, the XPS spectra are fitted to reveal two main peaks. Prior to fitting, a Shirley-type background was subtracted from each Zn 2p3/2 spectrum, and binding energies were calibrated against the C 1s peak at 284.9 eV (Section 2.3). Each spectrum was deconvoluted into two Gaussian components corresponding to ZnO and Zn(OH)+ species.

Fig. 7. XPS Spectrum (a) Zn Spectra, (b) Cr & Ni Spectra.

Fig. 7

The peak with lower binding energy (1023.1, 1022, 1022.2 for Zn@ZC, Zn@DS/ZC, and Zn@PVP/ZC, respectively) is attributed to ZnO, while a peak with higher binding energy (1024.7, 1024.2, 1024.1 for Zn@ZC, Zn@DS/ZC, and Zn@PVP/ZC, respectively) is assigned to Zn(OH)+ species, which have a stronger interaction with the parent zeolite framework. Literature76,77 confirms that the high binding energy peak corresponds to Zn(OH)+ species, formed through the strong interaction between zinc species and protonic acid sites. The Zn species peaks for ZnCr@PVP/ZC and ZnNi@PVP/ZC are identical to those of Zn@PVP/ZC, indicating that adding a second metal promoter does not change the peak positions.

The XPS results further reveal that the surface distribution of Zn species in the zeolite samples is strongly influenced by the synthesis route (Table 2). In the conventional Zn@ZC catalyst, most of the surface Zn exists as ZnO (73.9%), while the proportion of hydroxylated Zn(OH)+ species is relatively low (26.1%). A similar distribution is observed in the desilicated sample, with 70.5% ZnO and 29.5% Zn(OH)+, indicating that the desilication process has little effect on the oxidation state or dispersion of Zn species. In contrast, the Zn@PVP/ZC catalyst shows a markedly different behavior, with 32.8% ZnO and a dominant fraction of 67.2% Zn(OH)+ species.

This significant increase in hydroxylated Zn species can be attributed to the PVP-assisted synthesis, where the polymer-derived mesopores provide an expanded external surface and abundant silanol (Si–OH) groups capable of anchoring Zn2+ ions as hydroxylated cations during crystallization. The polar pyrrolidone units of PVP can coordinate with Zn2+ through their carbonyl and amide functionalities, which likely suppresses ZnO nucleation and promotes the dispersion of isolated Zn–OH moieties within the zeolite framework. Consequently, Zn species are predominantly present as well-dispersed Zn(OH)+ sites rather than aggregated ZnO clusters.

Furthermore, the XPS results indicate distinct distributions of surface Zn species depending on the secondary metal. The relative fractions of ZnO and Zn(OH)+ are 40.9% and 59.1% for ZnCr@PVP/ZC, and 12.7% and 87.3% for ZnNi@PVP/ZC, respectively. This comparison clearly shows that the Ni co-modified catalyst contains a much higher proportion of hydroxylated Zn(OH)+ species than its Cr counterpart. The enhanced formation of Zn(OH)+ in the presence of Ni can be attributed to the strong interaction between Ni and Zn, which favors the stabilization of framework-bound Zn(OH)+ moieties and simultaneously suppresses ZnO cluster formation, consistent with previous findings.78 Ni typically exists as Ni2+ or Ni0 species capable of electronic or structural interaction with Zn, thereby enhancing Zn dispersion and incorporation. In contrast, Cr is mainly incorporated as Cr3+ oxide (Cr2O3) or as mixed Zn–Cr spinel phases (e.g., ZnCr2O4). These CrOx species are relatively inert under reductive conditions and, therefore, less effective in promoting the generation of Zn(OH)+ sites.79

The Ni and Cr XPS spectra are shown in Fig. 7b. Ni exhibits binding energies at 851.1 eV and 856.2 eV, which are attributed to Ni0 and NiOH+, respectively. A satellite peak at 861.5 eV binding energy is assigned to Ni2+, consistent with the literature.63 Also, the binding energies of Cr 2p3/2 and Cr 2p1/2 were located at 575.0 eV and 585.26 eV, respectively, which could be assigned to Cr+3 in Cr2O3.14 In addition, 577.7 eV and 587.1 eV may correspond to the binding energies of Cr+6.64

Comparing ICP bulk Zn loading with the XPS-derived Zn(OH)+ fraction shows that the conventional and desilicated samples, with the lowest ICP Zn loadings (0.70–0.73 wt%), also show the lowest Zn(OH)+ fractions (26.1–29.4%), whereas all three PVP-templated samples, despite only modestly higher bulk Zn loadings (0.82–0.93 wt%), show substantially higher Zn(OH)+ fractions (59.9–87.4%). This indicates PVP-assisted synthesis improves the quality of Zn dispersion, not merely the quantity incorporated. Notably, ZnCr@PVP/ZC and ZnNi@PVP/ZC contain nearly identical promoter loadings by ICP (0.91 wt% Cr, 0.92 wt% Ni) yet show markedly different Zn(OH)+ fractions (59.9% vs. 87.4%), demonstrating that the specific redox chemistry of the secondary promoter, rather than its loading level, governs Zn speciation.

Notably, the Zn 2p3/2 peak positions remain unchanged upon Ni or Cr incorporation, indicating that the promoter effect is transmitted to Zn as a redistribution between the ZnO and Zn(OH)+ environments rather than as a shift in Zn binding energy. This redistribution tracks closely with the redox character of each promoter revealed by its own XPS signature: the low-binding-energy, electron-enriched Ni0 component (851.1 eV, below the ∼852.6 eV typical of bulk metallic Ni) is consistent with Ni acting as a local electron/hydrogen donor that favors conversion of ZnO into framework-anchored Zn(OH)+, whereas the coexistence of Cr3+ and a more oxidized Cr species (577.7/587.1 eV) indicates an electron-accepting character for Cr that does not drive the same transformation. This electronic coupling, rather than acid-site density alone, offers a mechanistic rationale for the markedly different Zn(OH)+ fractions obtained with Ni versus Cr promotion (87.4% vs. 59.9%, Table 2).

The XPS-derived Zn(OH)+ fractions correlate directly with catalytic performance (Table 4). Non-templated samples have the lowest Zn(OH)+ fractions (26.1–29.4%) and BTX selectivities (32.4–38.9%), whereas the PVP-templated series has substantially higher Zn(OH)+ fractions (59.9–87.4%) and correspondingly higher BTX selectivities (50.4–67.9%). ZnNi@PVP/ZC achieves the highest values for both Zn(OH)+ fraction (87.4%) and BTX selectivity (67.9%) in the series. These results position surface Zn speciation, rather than Zn loading or crystallinity alone, as the dominant XPS-derived descriptor of catalytic performance in this system.

3.1.6. NH3-TPD analysis

The NH3-TPD profiles and data were fitted using Gaussian methods, as illustrated in Fig. 8 and summarized in Table 3. Following linear baseline correction, each NH3-TPD desorption profile was deconvoluted into two Gaussian components. The integrated area of each Gaussian component was converted to an ammonia-desorption quantity (mmol g−1) using the total NH3 uptake determined during the saturation step (Section 2.3) as the calibration reference. This two-peak deconvolution was applied consistently across all five catalysts.

Fig. 8. NH3-TPD profiles.

Fig. 8

The desorption temperatures indicate whether each curve corresponds to weak or strong acid sites. The area under each curve reflects the amount of acid sites and is detailed in Table 3. Desorption at 150–300 °C is linked to physisorbed NH3 from weak acid sites, while desorption above 300–450 °C relates to stronger acid sites.26,36 According to the literature,50,80 weak acid sites are caused by Al species in extra-framework and non-framework positions (such as Si–OH–Al in structural defects). Conversely, strong acid sites are typically introduced by framework Al.

The NH3-TPD results reveal apparent differences in acidity among the synthesized samples (Table 3). The microporous Zn@ZC sample exhibits a total acidity of 0.692 mmol g−1, consisting of 0.393 mmol g−1 weak and 0.299 mmol g−1 strong acid sites. Upon desilication, the weak acid sites slightly increase to 0.431 mmol g−1, whereas the strong acid sites decrease to 0.285 mmol g−1. This behavior can be attributed to the alkaline treatment, which removes framework silicon and induces partial dealumination due to framework damage.81 Consequently, although the Si/Al ratio decreases and the total acidity rises, the strong acidity fraction diminishes.

In contrast, the PVP-assisted Zn@PVP/ZC sample displays the highest acidity, with weak and strong acid site densities of 0.455 and 0.490 mmol g−1, respectively. The presence of PVP generates mesoporosity, enhancing the accessibility and distribution of acid sites.82,83 Moreover, PVP interacts strongly with Al species during crystallization, directing more Al into framework positions and thus increasing the total acidity. This improvement likely arises from electronic interactions between PVP-coordinated metal species and the zeolite framework, facilitating the creation of additional strong and weak acid sites.

The introduction of secondary metal promoters further modifies the acid distribution. Incorporation of Ni increases the weak-site NH3 uptake from 0.455 to 0.563 mmol g−1 while reducing the strong-site uptake from 0.490 to 0.381 mmol g−1. This indicates that Ni promotes the transformation of strong acid sites into weaker ones without significantly altering the total acidity.84 The effect can be attributed to the partial substitution of framework protons by Ni2+ ions, which have a lower charge density and therefore weaken the electrostatic interaction with framework oxygen atoms.

Accordingly, the desorption maxima of the deconvoluted components shift. Compared with Zn@PVP/ZC (201 and 382 °C for the weak and strong components, respectively), Ni incorporation lowers the maxima by 11 °C (to 190 °C) and 24 °C (to 358 °C). Thus, Ni not only converts strong acid sites into weak ones but also lowers the desorption temperature—and therefore the strength—of both site populations. This is consistent with the partial replacement of framework protons by Ni species with lower charge density.

Conversely, Cr addition leads to a pronounced decrease in weak acidity and a slight reduction in strong acidity, resulting in the dominance of strong acid sites. This trend contrasts with previous reports,85,86 where Cr incorporation was found to reduce both weak and strong acidity but retained a higher proportion of weak sites. In the present work, the reverse behavior suggests that Cr incorporation does not generate new compensating weak acid sites, possibly because Cr species occupy or neutralize existing Brønsted acid positions within the zeolite framework.

Additionally, Cr incorporation shifts both desorption maxima to higher temperatures than those of Zn@PVP/ZC: by 62 °C for the weak component (201 → 263 °C) and by 31 °C for the strong component (382 → 413 °C). After Cr incorporation, the acid sites are fewer but more strongly bound, consistent with the introduction of Cr3+/Cr6+ oxide species, which add strongly bound acidity rather than replace Brønsted sites. Across this catalyst series, the Ni-induced decrease and Cr-induced increase in the desorption maxima therefore parallel the rise in the strong-to-weak ratio from ZnNi@PVP/ZC to ZnCr@PVP/ZC (0.68 → 1.56).

3.2. MTA catalytic performance

ZSM-5 zeolites are well known for their exceptional physicochemical properties, which make them highly effective catalysts for methanol-to-hydrocarbon (MTH) conversion. In this study, all synthesized Zn-modified ZSM-5 catalysts were evaluated for their performance in methanol aromatization. As shown in Table 4, the product selectivity data at 3 h time-on-stream (TOS) indicate that methanol conversion remains consistently above 99.5% during the reaction, demonstrating excellent catalytic stability. The microporous Zn@ZC exhibits aromatic selectivity of 39.5% and BTX selectivity of 32.4%. Due to the incorporation of Zn into ZSM-5, this sample exhibits greater aromatic selectivity compared to the non-metal-modified sample previously studied.8,75

However, the selectivity of C2–C4 alkanes is 38%. The high selectivity toward light alkanes suggests that the reaction predominantly follows cracking pathways, in which C–C bond cleavage becomes more favorable than chain growth, leading to the formation of alkane hydrocarbons. This behavior is typical of ZSM-5's microporous structure, which may create diffusion constraints, especially for larger intermediates and products, possibly obstructing their further conversion into aromatics.

The alkali-treated Zn@DS/ZC catalyst exhibits enhanced aromatic and BTX selectivity, reaching 53.7% and 43.9%, respectively. This improvement can be correlated with the increased textural properties, where the surface area (SBET) and total pore volume rise from 300.2 m2 g−1 to 342.4 m2 g−1 and from 0.173 cm3 g−1 to 0.304 cm3 g−1, respectively. The generation of mesoporosity facilitates molecular diffusion and enhances the accessibility of reactant molecules to active sites within the microporous channels, thereby promoting aromatic selectivity.

However, excessive NaOH leaching, although effective in creating mesopores, also induces severe structural damage and framework defects, resulting in a loss of shape selectivity. Consequently, the formation of larger carbon chains and an increased selectivity toward C9+ hydrocarbons are observed compared to the parent Zn@ZC sample. This process also results in a decrease in strong acid sites, as confirmed by the NH3-TPD data (Table 3). The reduction in strong acidity suppresses hydrogen transfer and alkane formation, while favoring light olefin (C2–C4 Created by potrace 1.16, written by Peter Selinger 2001-2019 ) production. Nevertheless, this modification does not lead to a significant improvement in BTX selectivity.

The Zn@PVP/ZC catalyst shows significantly higher aromatics (67.3%) and BTX (61.8%) selectivity compared to Zn@ZC. This improvement mainly results from the formation of a well-developed hierarchical structure induced by the PVP template. BET and BJH analyses indicate that Zn@PVP/ZC has uniform mesoporosity (Vmeso = 0.179 cm3 g−1) while preserving its inherent microporous framework (Vmicro = 0.097 cm3 g−1). These hierarchical textural features enhance molecular diffusion and increase access to active acid sites, promoting aromatization over secondary reactions. Additionally, the increased concentration and balanced distribution of both strong and weak acid sites create a more favorable environment for the formation of BTX. PVP addition also improves the dispersion of Zn species, reduces structural defects, prevents ZnO aggregation, and maintains the integrity of the zeolitic framework. Consequently, the synergistic effect of hierarchical porosity, optimized acidity, and uniform metal dispersion results in a higher BTX yield and lower production of heavy aromatic byproducts (C9+) compared to the desilicated Zn@DS/ZC sample. In another aspect, the state of Zn particle is a critical parameter in the MTA reaction.

In the Cr-promoted sample, the incorporation of chromium appears to alter the acid site distribution significantly. The overall acidity is lower than that of Zn@PVP/ZC, which likely contributes to the lower aromatic and BTX selectivity observed. Moreover, the increased proportion of strong to weak acid sites promotes excessive cracking and hydrogen transfer reactions, favoring the formation of undesired products such as alkanes and heavy C9+ aromatics. As a result, the selectivity for alkanes and C9+ aromatics increases from 15.5% to 22.8% and from 5.5% to 10%, respectively.

The ZnNi@PVP/ZC sample maintains a similar morphology and structural integrity to Zn@PVP/ZC but exhibits notably higher aromatic selectivity, with BTX selectivity increasing to 67.9%. The incorporation of Ni appears to stabilize a greater amount of Zn species within the zeolite framework, which in turn facilitates the conversion of strong acid sites into weaker ones. This modification enhances dehydration and aromatization pathways, ultimately leading to the improved BTX selectivity observed.

The carbon-based space-time yield (STY) values provide a productivity-based perspective that complements the selectivity data in Table 4. Zn@ZC, despite its purely microporous structure, exhibits the lowest STY for both aromatics (1.97 gC gcat−1 h−1) and BTX (1.61 gC gcat−1 h−1), due to its high selectivity for light alkanes over aromatics. Desilication slightly enhances productivity (2.57 and 1.94 gC gcat−1 h−1), but PVP-templated samples show a more significant improvement: Zn@PVP/ZC nearly doubles the aromatic and BTX STY compared to Zn@ZC (3.35 and 3.07 gC gcat−1 h−1). Among the bimetallic catalysts, ZnNi@PVP/ZC achieves the highest overall productivity, with 3.57 gC gcat−1 h−1 for aromatics and 3.38 gC gcat−1 h−1 for BTX. Although ZnCr@PVP/ZC, with its hierarchical structure, produces slightly lower STYs (3.04 and 2.51 gC gcat−1 h−1) than Zn@PVP/ZC, its lower selectivity towards the target products explains this difference. Since methanol conversion remains effectively constant (>99.5%) across all catalysts, the differences in STY closely follow the trends in selectivity. Nevertheless, expressing performance as an absolute productivity proves that enhancements from PVP-assisted hierarchical structuring and Ni promotion genuinely increase the amount of aromatics and BTX produced per unit catalyst per unit and time, rather than merely shifting the product distribution.

To clarify how hierarchical porosity and Zn dispersion individually influence BTX selectivity, the catalyst pairs were examined in which one factor is significantly changed while the other remains approximately constant. Between Zn@ZC and Zn@DS/ZC, the mesopore volume fraction (Vmeso/Vtotal) increases dramatically from 6.9% to 67.1%, while the Zn(OH)+ fraction varies only slightly (26.1% to 29.4%). This porosity-driven change results in a modest BTX improvement (32.4% to 38.9%). Conversely, between Zn@DS/ZC and Zn@PVP/ZC, the mesopore fraction remains nearly constant (67.1% vs. 64.9%), but the Zn(OH)+ fraction increases sharply (29.4% to 67.2%), leading to a much larger BTX increase (38.9% to 61.8%). An additional rise in Zn(OH)+ alone (67.2% to 87.4%, from Zn@PVP/ZC to ZnNi@PVP/ZC, with little change in mesopores) further boosts BTX selectivity. Overall, these comparisons show hierarchical mesoporosity is essential, but Zn(OH)+/ZnO speciation mainly drives BTX selectivity. This asymmetry in impact aligns with the different functions of the two factors in the reaction process. Mesoporosity mainly affects transport by reducing diffusion lengths and facilitating access of reactants and intermediate molecules to acid sites within the crystal without changing the chemical nature or intrinsic reactivity of those sites. Therefore, increasing mesoporosity, with the Zn(OH)+/ZnO ratio unchanged (as seen in the Zn@ZC to Zn@DS/ZC comparison), mainly mitigates diffusion constraints in a reaction pathway still dominated by hydrogen transfer, resulting in only a modest increase in BTX yield. Conversely, Zn(OH)+ species serve as active sites that catalyze dehydrogenation, directly enhancing alkene/alkane dehydrogenation while suppressing the competing hydrogen-transfer route that produces light alkanes and heavier alkyl aromatics. Increasing the Zn(OH)+ content thus not only improves access to existing chemistry but also fundamentally alters the chemistry at active sites, shifting more of the reaction network toward aromatization/BTX formation. Since this shift affects the rate- and selectivity-determining step rather than transport, it has a much larger impact on BTX selectivity than porosity alone. This explains why hierarchical mesoporosity is essential as an enabling factor, while the Zn(OH)+/ZnO speciation primarily determines the extent of BTX selectivity across the catalyst series.

3.2.1. Morphology properties' effect on the MTA performance

The reactor test results for methanol-to-aromatics conversion, in conjunction with the morphological features of the synthesized zeolitic catalysts, show that, as expected, mesoporous samples exhibit catalytic performance. Their larger pore volume, increased accessible surface area, and enhanced diffusion pathways enable more extensive contact between methanol molecules and acid sites, resulting in higher overall aromatic selectivity. However, among the mesoporous catalysts, morphology alone does not seem to be the main factor influencing performance.

The connection between particle size and MTA performance shown in Fig. 9 becomes clearer when analyzing how each variable changes across the catalyst series.

Fig. 9. Effect of particle size on MTA performance.

Fig. 9

When the average particle size decreases from 20.2 µm (Zn@DS/ZC) to 6.7 µm (Zn@PVP/ZC), BTX selectivity significantly increases from 38.9% to 61.8%. Further reduction to 2.37 µm (ZnNi@PVP/ZC) results in the highest BTX selectivity at 67.9%, a +6.1point increase from Zn@PVP/ZC. This pattern aligns with the idea that smaller particles facilitate easier exit of aromatic intermediates before secondary alkylation produces heavier, less desired products. However, ZnCr@PVP/ZC deviates from this trend: despite being smaller (4.5 µm) than Zn@PVP/ZC (6.7 µm), its BTX selectivity is lower (50.4% vs. 61.8%).

This exception shows that reducing particle size alone does not guarantee improve BTX selectivity. Instead, the acid-site chemistry plays a crucial role, sometimes outweighing the benefits of smaller crystals. Overall, reducing particle size generally supports higher BTX selectivity through improved diffusion, but this benefit can be negated when the acid-site environment promotes condensation and dealkylation pathways over methylation and dealkylation toward xylenes.

3.2.2. Zn state effect on the MTA performance

During the MTA process, methanol molecules adsorb onto the catalyst surface and are converted into intermediate olefin products at strong acid sites. These products then undergo a series of tandem reactions, such as dehydrogenation, hydrogen transfer, and cyclization, ultimately forming aromatic compounds. Adding zinc can improve the dehydrogenation of alkanes and the aromatization of alkenes, while also reducing the formation of light alkanes. This is because Zn weak acid sites, originating from ZnOH+ species, can diminish strong acid sites and thus inhibit hydrogen-transfer reactions.76,77 Additionally, Niu et al. highlighted that ZnOH+ acts as a catalytically active species in the dehydrogenation of olefinic intermediates.76 Conversely, it has been shown that ZnO species are less effective at aromatizing alkanes.

Besides its link to overall BTX selectivity, the role of Zn(OH)+ in promoting dehydrogenation is clear in its effect on the competing hydrogen-transfer pathway. Effective dehydrogenation should reduce the formation of C2–C4 paraffins, which are direct products of hydrogen-transfer reactions. The data shows that as the Zn(OH)+ fraction rises across the catalyst series, the C2–C4 alkane selectivity (Table 4) consistently drops, from 38.0% (Zn@ZC, 26.1% Zn(OH)+) to 15.3% (ZnNi@PVP/ZC, 87.4% Zn(OH)+). Supported by XPS speciation, this trend suggests that higher Zn(OH)+ levels inhibit hydrogen-transfer pathways that produce alkanes, instead promoting aromatization and BTX formation. As shown in Fig. 10, there is a clear linear relationship between the fraction of Zn(OH)+ species and the selectivity toward aromatics and BTX.

Fig. 10. Effect of Zn state on MTA performance.

Fig. 10

Increasing the proportion of Zn(OH)+ from 29.4% in Zn@DS/ZC to 67.1% in Zn@PVP/ZC results in an approximately 63% increase in BTX selectivity, highlighting the key role of these species in directing aromatic formation. A similar pattern appears with the bimetallic catalysts: a reduction of Zn(OH)+ in ZnCr@PVP/ZC leads to lower aromatic and BTX selectivity, while promoting Zn(OH)+ through Ni addition—aligning with the mechanism discussed in Section 3.1.5—restores and further improves aromatic productivity. Among all catalysts, ZnNi@PVP/ZC exhibits the highest Zn(OH)+ levels and BTX selectivity.

These findings suggest that although the morphology of the bimetallic samples is similar, the abundance of Zn(OH)+ species primarily determines catalytic performance in the MTA process.

3.2.3. Acidity effect on aromatic distributions

Fig. 11 displays aromatic distribution corresponding to the strong-to-weak acidity ratio (mentioned as S/W). The balance between strong and weak acid sites within the zeolitic framework strongly affects the distribution of aromatic products. The ratio of benzene, toluene, xylenes, and C9+ aromatics to total aromatics is defined as B/A, T/A, X/A, and C9+/A, respectively.

Fig. 11. Strong to weak acid ratio on aromatic distribution.

Fig. 11

For the single-metal Zn-modified sample with the highest amount of strong and weak acidity and an S/W ratio of about 1, toluene and Xylene are the main products, accounting for 31.9% and 49.3%, respectively. Also, the portion of heavy C9+ aromatics is about 8.2%.

Adding a second transition metal to Zn@PVP/ZC significantly alters the distribution of aromatic products. The ZnNi-modified sample shows the highest xylene fraction (61.8%) and the most significant overall BTX proportion. In contrast, ZnCr produces a larger share of heavy C9+ aromatics (17.5%) and the highest measured strong/weak (S/W) acid ratio.

These trends suggest that both the acid site distribution (S/W ratio) and the metal–zeolite synergy determine whether the network favors methylation/dealkylation toward xylenes or deeper cracking and retention of heavier aromatics. Notably, incorporating Zn creates ZnOH+ sites that promote dehydrogenation and primary aromatization while inhibiting extensive hydrogen transfer; this behavior increases the pool of alkylated aromatics available for secondary alkylation/dealkylation. Adding Ni further stabilizes the Zn species (reducing Zn loss) and boosts dehydrogenation activity, and aligns with previous findings showing that Ni can facilitate the methylation of toluene, promoting its transformation into xylenes. Besides, the proportion of heavy aromatics decreases in the Ni-containing catalyst, which can be attributed to a reduced density of strong acid sites, which typically drive excessive chain growth and the formation of C9+ aromatics.

The influence of a higher S/W ratio (as seen with ZnCr@PVP/ZC) appears more complex: increased strong acidity promotes protolytic dealkylation and can lead to a greater proportion of C9+ residues. In other words, a moderate S/W ratio combined with Zn-derived Lewis sites and Ni-enhanced dehydrogenation offers the best selectivity for higher-value xylenes, while much stronger acidity pushes the network toward deeper rearrangement and higher-boiling alkylbenzenes.

The magnitude of these shifts, a threefold change in C9+ fraction and approximately a 20-percentage-point variation in xylene fraction over a relatively narrow S/W range (0.68–1.56), highlights that the acid-site balance, rather than just the total amount of acid, is a key factor controlling the extent of alkylation and the composition of aromatic products in this catalyst series.

Within this series, S/W increases monotonically from ZnNi@PVP/ZC (0.68) to Zn@PVP/ZC (1.08) to ZnCr@PVP/ZC (1.56), and this ranking is mirrored exactly by C9+ selectivity (3.9%, 5.5%, 10.7%) and by both total and internally confined coke mass (40.0 mg/46.7% internal; 73.3 mg/59.4% internal; 77.2 mg/66.2% internal), and inversely by BTX selectivity (67.9%, 61.8%, 50.4%). This indicates that an excess of strong acid sites promotes secondary cracking and condensation reactions that generate C9+ byproducts and hydrogen-deficient coke precursors, which preferentially accumulate within the microporous network and progressively restrict access to active sites.

3.2.4. MTA performance time on stream data of bimetal hierarchical ZSM-5

The time-on-stream profiles reveal selectivity patterns among the PVP metal-modified catalysts (Fig. 12). Zn@PVP/ZC shows a gradual decrease in BTX selectivity (from 61.8% to 43.4%), alongside increased C9+ formation. Additionally, methanol conversion drops to 96.3%. In contrast, ZnCr@PVP/ZC experiences the fastest decline in BTX selectivity (from 50.4% to 26.9%) and the most significant rise in heavy C9+ aromatics (up to 22.1%). This swift decline is linked to its higher strong/weak acidity ratio and the known tendency of Cr–Zn systems to promote polyalkylation and condensation reactions that produce polyaromatic coke precursors.

Fig. 12. MTA performance time on stream of PVP-metal modified samples.

Fig. 12

Literature indicates that high strong acidity can facilitate aromatic condensation, oligomerization, and poly-methylbenzene formation—well-known pathways for rapid catalyst deactivation in MTA. This aligns with the observed higher C9+ residues and lower BTX yields in the Cr-containing catalyst. The best stability is observed with ZnNi@PVP/ZC, which maintains higher BTX selectivity (around 67.9% to 54.8%) and significantly less C9+ buildup than the other catalysts.

To quantify how shorter internal diffusion paths affect TOS stability, the three PVP-templated catalysts were compared, which have nearly identical mesopore volume fractions (64.2–64.9%, Table 1). Despite this similarity—and despite ZnCr@PVP/ZC having a smaller average particle size (4.5 µm) than Zn@PVP/ZC (6.7 µm, Fig. 9)—ZnCr@PVP/ZC shows the lowest BTX retention after 10 h on stream, at 53.4% of its initial value, compared with 70.2% for Zn@PVP/ZC and 80.7% for ZnNi@PVP/ZC. Thus, shorter diffusion paths alone do not ensure TOS stability. Instead, BTX retention decreases monotonically as the absolute mass of coke trapped in the micropore network increases. Calculated from the total coke mass and internal coke fraction in Table 5, these masses are 18.7 mg (ZnNi@PVP/ZC) < 43.5 mg (Zn@PVP/ZC) < 51.1 mg (ZnCr@PVP/ZC)—the exact inverse order of BTX retention. Mesoporosity therefore creates a structural opportunity for coke precursors to escape before pore blockage occurs, but promoter-dependent acid/redox chemistry determines how fully that opportunity is realized (Section 3.1.5). In this series, internal coke mass—not mesopore fraction alone—is the direct quantitative link to TOS stability.

The improved performance results from the synergistic interaction between Ni and Zn: Ni stabilizes Zn against volatilization and restructuring, boosts dehydrogenation, increases aromatic precursor formation, supplies hydrogen to suppress polyaromatic coke nuclei, and sustains the methylation/dealkylation network. This combination effectively delays intracrystalline coking, consistent with the slower decline in BTX activity. Overall, the TOS comparison shows that: (1) ZnNi synergy offers superior resistance to deactivation, (2) Cr enhances acidity and condensation pathways, leading to rapid aromatization loss, and (3) Zn alone has moderate performance, with typical aromatization selectivity but limited long-term stability due to coke buildup.

3.2.5. Coke formation

Thermogravimetric (TG) analysis was used to assess carbon deposition on the catalysts after the MTA reaction. Fig. 13 presents the TG profiles, while Table 5 provides coke data for all catalysts post-reaction. Additionally, the changes in micropore and external surface areas are indicated as ΔSmicro and ΔSmeso, respectively, and are displayed in Fig. 14.

Fig. 13. TGA profile of the spent catalysts.

Fig. 13

Fig. 14. Reduction in the micropore and external area of the spent catalysts.

Fig. 14

The calculations indicated that the percentage weight loss for the catalysts was 6.95% for Zn@ZC, 5.39% for Zn@DS/ZC, 4.63% for Zn@PVP/ZC, 4.4% for ZnCr@PVP/ZC, and 2.4% for ZnNi@PVP/ZC. Despite its smallest surface area and pore volume, the Zn@ZC catalyst produces and retains the largest quantity of coke due to its microporous structure. Its dominant internal deposition (82.6%) corresponds to the largest loss in micropore area, confirming that diffusion-limited microporous environments trap bulky aromatic intermediates, which subsequently evolve into internal coke, in agreement with literature showing that internal coking can lead to faster deactivation because the coke blocks the strong acid sites and diffusion through the micropores.39

Quantitatively, Zn@ZC exhibits the largest overall surface-area reduction after reaction (∼63.5%), of which the great majority (∼52.5 percentage points) arising from micropore area (ΔSmicro). This confirms that in the absence of mesoporosity, coke formation and pore blockage occur almost exclusively within the microporous network. The two bimetallic catalysts have nearly identical fresh external surface areas and pore volumes. Of these, ZnNi@PVP/ZC shows the smallest total surface-area loss (∼30%) and a nearly even ΔSmicro/ΔSmeso split (∼14.5%/∼15.5%). By contrast, ZnCr@PVP/ZC shows a considerably larger total loss (∼53.5%), weighted toward micropore area loss (ΔSmicro ≈ 35.5% vs. ΔSmeso ≈ 18%). This pre-/post-reaction textural comparison directly and independently confirms the metal-specific localization trend inferred from the coke-mass data in Table 5: Ni promotion preferentially preserves the micropore network by directing coke toward the external surface, whereas Cr promotion allows coke accumulation to erode the micropore structure more extensively.

By contrast, desilicated and PVP-templated samples (Zn@DS/ZC and Zn@PVP/ZC) exhibit significantly lower total coke (89.8 and 73.3 mg) and a marked shift toward external deposition (34.5–40.6%), consistent with their larger mesoporous contribution (ΔSmeso increase), which facilitates Because of their greater external surface area and shorter diffusion path, coke precursors generated in micropores easily moved to the external surface. Although Zn@DS/ZC possesses a larger surface area and pore volume than Zn@PVP/ZC, it nevertheless exhibits higher coke deposition. This behavior may be attributed to the greater structural defects generated during the desilication treatment, which favor coke formation. ZnCr@PVP/ZC shows 77.2 mg coke and a relatively high internal fraction (66.2%), reflecting the effect of increased strong acidity known to promote aromatic condensation.

This behavior matches reports68,87 that excessive acidity accelerates internal coking even in hierarchical zeolites. Notably, ZnNi@PVP/ZC displays the lowest coke amount (40.0 mg) and the highest fraction of external coke (53.3%), consistent with its smallest ΔSmicro/ΔSmeso ratio. This performance arises from the Zn–Ni synergy, where Ni-assisted dehydrogenation, potentially accompanied by hydrogen spillover, is proposed to suppress hydrogen-deficient PAH nucleation within micropores and favor coke accumulation on the external surface, where it is less detrimental to diffusion.10 Collectively, the combined TGA and porosity trends confirm that introducing mesoporosity and an acidity distribution, with Ni-induced shifts, and coke deposition from internal to external regions drastically reduces overall coking rates, thereby enhancing catalyst longevity. Analyzing the coke data alongside the initial textural properties listed in Table 1 offers deeper understanding of this behavior. ZnNi@PVP/ZC and ZnCr@PVP/ZC have almost identical initial external surface areas (70.4 vs. 69.5 m2 g−1) and total pore volumes (0.248 vs. 0.246 cm3 g−1), yet their coke outcomes vary significantly: ZnNi@PVP/ZC retains only 40.0 mg of coke, with 53.3% on the external surface, whereas ZnCr@PVP/ZC retains nearly twice as much (77.2 mg), with most (66.2%) trapped internally. This comparison shows that initial pore texture alone does not explain differences in coke amount or distribution between these two bimetallic catalysts; instead, the metal-specific chemistry, Ni-facilitated dehydrogenation and with spillover proposed as a contributing mechanism, versus strong acidity promotion and aromatic condensation by chromium, determines whether coke precursors are directed to the external surface or confined within the microporous network.

A similar contrast appears between Zn@DS/ZC and Zn@PVP/ZC: even though Zn@DS/ZC has a higher BET surface area and total pore volume (373.6 vs. 333.1 m2 g−1; 0.329 vs. 0.276 cm3 g−1), it retains more coke (89.8 vs. 73.3 mg) but exhibits a smaller fraction of coke on the external surface (34.5% vs. 40.6%). This underscores that textural capacity alone does not determine coke behavior and that structural defects caused by desilication likely contribute to the increased coke in Zn@DS/ZC, despite its initially more favorable texture.

To quantify coke reactivity beyond the previously discussed TGA analysis, apparent activation energies for coke combustion were calculated using the Coats–Redfern method.67 Zn@ZC and Zn@DS/ZC exhibit activation energies of 23.2 and 24.2 kJ mol−1, respectively, suggesting that alkaline desilication primarily redistributes coke between internal and external surfaces and decreases its total amount, without significantly changing its intrinsic chemical reactivity. Conversely, Zn@PVP/ZC shows the highest activation energy at 34.9 kJ mol−1, implying a more thermally resistant, possibly more condensed and hydrogen-deficient coke, despite its much lower overall coke quantity compared to Zn@ZC and Zn@DS/ZC. This decoupling between coke quantity and reactivity indicates that these properties are influenced by at least partly separate factors—pore structure primarily limits coke accumulation, while the local acid-site environment influences the extent of dehydrogenation and condensation of coke precursors before trapping. ZnCr@PVP/ZC's activation energy of 25.6 kJ mol−1 aligns with its higher strong-acid density, which promotes further dehydrogenation and aromatic condensation of coke precursors, consistent with reports that coke with a lower H/C ratio forms a more condensed, less reactive deposit requiring higher activation energy for combustion.86 In contrast, ZnNi@PVP/ZC has a low activation energy of 23.8 kJ mol−1, similar to Zn@ZC, and exhibits the smallest total coke amount along with the highest external coke fraction among all catalysts. This combination suggests that coke on ZnNi@PVP/ZC is limited and easier to oxidize, which benefits catalyst regeneration and reduces diffusion resistance in the micropore network. Considering the pre-exponential factor alongside Ea reveals a strong compensation relationship across the series, a pattern widely reported in solid-state and coke-combustion kinetics. This means that the ∼12 kJ mol−1 range in apparent activation energy across the catalysts does not translate into an equally large difference in intrinsic oxidation rate: catalysts with higher Ea also have proportionally higher A values. Comparing the two bimetallic formulations, both Cr and Ni promotion reduce coke activation energy relative to the monometallic Zn@PVP/ZC parent (by 9.3 and 11.1 kJ mol−1, respectively), but do so differently. ZnCr@PVP/ZC retains a relatively large, internally confined coke deposit (77.2 mg, 66.2% internal) with a lower activation energy than the parent catalyst. By contrast, ZnNi@PVP/ZC combines the lowest Ea in the series with the smallest total coke mass (40.0 mg) and the highest external coke fraction (53.3%). This is consistent with coke that is both minimal in quantity and intrinsically easier to combust, favoring catalyst regenerability.88

This behavior is similar to previous findings in hierarchical versus microporous ZSM-23 zeolites, where hierarchical structures reduced both coke deposition and activation energy for oxidation, lowering the energy required for regeneration.89

4. Conclusion

Below is a summary of our study's findings:

(1) In this study, we developed a one-pot PVP-assisted synthesis strategy to prepare hierarchical Zn-modified ZSM-5 catalysts, followed by incorporating Ni and Cr as secondary metal promoters. Comprehensive characterization demonstrated that PVP promoted the formation of a hierarchical micro–mesoporous architecture while facilitating Zn dispersion and increasing the fraction of surface Zn(OH)+ species.

(2) The catalytic results show that hierarchical porosity improves molecular accessibility and diffusion; however, mesoporosity alone does not fully determine MTA performance. For example, increasing the mesopore fraction from 6.9% in Zn@ZC to 67.1% in Zn@DS/ZC increased BTX selectivity by only 6.5 percentage points, from 32.4% to 38.9%.

(3) In contrast, Zn@PVP/ZC, which possesses a broadly comparable mesopore fraction (64.9%), exhibited a BTX selectivity of 61.8%, corresponding to a further increase of 22.9 percentage points. This comparison indicates that the chemical state of Zn and the balance of acid sites play a critical role in determining product selectivity in addition to hierarchical pore accessibility.

(4) The promoter identity strongly influenced Zn speciation and acidity, leading to distinct catalytic behavior. Ni promotion increased the Zn(OH)+ fraction to 87.4%, compared with 59.9% for the Cr-promoted catalyst, while shifting the acid-site distribution toward a lower strong-to-weak acidity ratio. This favorable combination enhanced BTX formation and suppressed coke deposition.

(5) Accordingly, ZnNi@PVP/ZC exhibited the highest BTX selectivity (67.9%) and the lowest coke amount (40.0 mg) among the investigated catalysts. In contrast, the Cr-promoted catalyst retained a higher contribution of strong acidity and a lower Zn(OH)+ fraction, which was accompanied by lower BTX selectivity and greater coke deposition.

(6) Overall, the results demonstrate that selective methanol aromatization over Zn-modified hierarchical ZSM-5 is governed by the combined effects of pore architecture, acid-site distribution, and Zn chemical state, with Ni promotion providing the most favorable balance for BTX-selective and coke-resistant operation.

Conflicts of interest

There are no conflicts to declare.

Data availability

The data supporting this article are available within the published article.

References

  1. Busca G. Production of gasolines and monocyclic aromatic hydrocarbons: from fossil raw materials to green processes. Energies. 2021;14:4061. doi: 10.3390/en14134061. [DOI] [Google Scholar]
  2. Maneffa A. Priecel P. Lopez-Sanchez J. A. Biomass-derived renewable aromatics: selective routes and outlook for p-xylene commercialisation. ChemSusChem. 2016;9:2736–2748. doi: 10.1002/cssc.201600605. [DOI] [PubMed] [Google Scholar]
  3. Li T. Shoinkhorova T. Gascon J. Ruiz-Martinez J. Aromatics production via methanol-mediated transformation routes. ACS Catal. 2021;11:7780–7819. doi: 10.1021/acscatal.1c01422. [DOI] [Google Scholar]
  4. Wang X. Yin Y. Li H. Fan S. Lv J. Zhao T. The effect of Ce promotor on catalytic performance of Zn/ZSM-5 in coaromatization of methanol and n-hexane. Microporous Mesoporous Mater. 2024;375:113158. doi: 10.1016/j.micromeso.2024.113158. [DOI] [Google Scholar]
  5. Ren X.-Y. Cao J.-P. Zhao S.-X. Zhao X.-Y. Liu T.-L. Feng X.-B. et al., Encapsulation Ni in HZSM-5 for catalytic hydropyrolysis of biomass to light aromatics. Fuel Process. Technol. 2021;218:106854. doi: 10.1016/j.fuproc.2021.106854. [DOI] [Google Scholar]
  6. Wang Y. Liu J. Zhao Z. Guo Q. Jiang Q. He N. et al., A carbon-negative route for sustainable production of aromatics from biomass-derived aqueous oxygenates. Appl. Catal. B. 2022;307:121139. doi: 10.1016/j.apcatb.2022.121139. [DOI] [Google Scholar]
  7. Ghanbari B. Zangeneh F. K. Rizi Z. T. Aghaei E. Highly efficient production of benzene-free aromatics from methanol over low-Si/Al-ratio alkali-modified Fe/Zn/HZSM-5. ACS Omega. 2018;3:18821–18835. doi: 10.1021/acsomega.8b01380. [DOI] [PMC free article] [PubMed] [Google Scholar]
  8. Zhou Y. Tang J. Chu R. Hu S. Chen S. Nie R. et al., Crafting Zn/nano-H-ZSM-5 catalysts for methanol-to-aromatics conversion: tailoring crystal size and modifying surface electron density. J. Mater. Chem. A. 2025;13:14189–14204. doi: 10.1039/D5TA01181G. [DOI] [Google Scholar]
  9. Fu T. Han Y. Li C. Guo M. Zhan G. Li Z. Self-assembly of hierarchical ZSM-5 particles on rice husk template as hybrid catalysts for boosting methanol aromatization. Chem. Eng. Sci. 2024;284:119457. doi: 10.1016/j.ces.2023.119457. [DOI] [Google Scholar]
  10. Jia Y. Wang J. Zhang K. Feng W. Liu S. Ding C. et al., Promoted effect of zinc–nickel bimetallic oxides supported on HZSM-5 catalysts in aromatization of methanol. J. Energy Chem. 2017;26:540–548. doi: 10.1016/j.jechem.2016.10.014. [DOI] [Google Scholar]
  11. Wang J. Jiang J. Sun Y. Wang X. Li M. Pang S. et al., Catalytic degradation of waste rubbers and plastics over zeolites to produce aromatic hydrocarbons. J. Cleaner Prod. 2021;309:127469. doi: 10.1016/j.jclepro.2021.127469. [DOI] [Google Scholar]
  12. Shen Y. Liu C. Cui C. Ren H. Gu M. Liu H. et al., Effect of Cu-modified HZSM-5 zeolites on catalytic pyrolysis of lignin to producing aromatic hydrocarbons. Fuel. 2024;361:130719. doi: 10.1016/j.fuel.2023.130719. [DOI] [Google Scholar]
  13. Wu L. Liu J. Chen L. Wang X. Zhou Q. Yu F. et al., Hierarchical beta zeolites assisted aromatics production from lignin via catalytic fast pyrolysis. Chem. Eng. J. 2024;484:149618. doi: 10.1016/j.cej.2024.149618. [DOI] [Google Scholar]
  14. Zhang L. Fu T. Ren K. Han Y. Wang R. Zhan G. et al., Finely regulating methanol concentration to control the alkylation depth in methanol aromatization for optimizing product distribution. Appl. Catal., B. 2023;321:122047. doi: 10.1016/j.apcatb.2022.122047. [DOI] [Google Scholar]
  15. Yang L. Liu Z. Liu Z. Peng W. Liu Y. Liu C. Correlation between H-ZSM-5 crystal size and catalytic performance in the methanol-to-aromatics reaction. Chin. J. Catal. 2017;38:683–690. doi: 10.1016/S1872-2067(17)62791-8. [DOI] [Google Scholar]
  16. Pan M. Jiang X. Pang Y. Pan X. Zhang Q. Yang R. et al., One-step synthesis of hierarchical ZSM-5 zeolites with low defect density as long-lived MTH catalysts. Appl. Catal., A. 2023;656:119132. doi: 10.1016/j.apcata.2023.119132. [DOI] [Google Scholar]
  17. Li H. Zhao Y. Ji D. Zhao X. Li C. Guo P. et al., Synthesis of hollow HZSM-5 zeolite-based catalysts and catalytic performance in MTA reaction. Microporous Mesoporous Mater. 2022;329:111546. doi: 10.1016/j.micromeso.2021.111546. [DOI] [Google Scholar]
  18. Shao J. Fu T. Ma Z. Zhang C. Li H. Cui L. et al., Facile creation of hierarchical nano-sized ZSM-5 with a large external surface area via desilication–recrystallization of silicalite-1 for conversion of methanol to hydrocarbons. Catal. Sci. Technol. 2019;9:6647–6658. doi: 10.1039/C9CY01053J. [DOI] [Google Scholar]
  19. Fu T. Wang Y. Li Z. Surface-Protection-Induced controllable restructuring of pores and acid sites of the nano-zsm-5 catalyst and its influence on the catalytic conversion of methanol to hydrocarbons. Langmuir. 2020;36:3737–3749. doi: 10.1021/acs.langmuir.0c00214. [DOI] [PubMed] [Google Scholar]
  20. Ghanbari B. Kazemi Zangeneh F. Taheri Rizi Z. Aghaei E. High-impact promotional effect of Mo impregnation on aluminum-rich and alkali-treated hierarchical zeolite catalysts on methanol aromatization. ACS Omega. 2020;5:11971–11986. doi: 10.1021/acsomega.9b04407. [DOI] [PMC free article] [PubMed] [Google Scholar]
  21. Zhang J. Qian W. Kong C. Wei F. Increasing para-xylene selectivity in making aromatics from methanol with a surface-modified Zn/P/ZSM-5 catalyst. ACS Catal. 2015;5:2982–2988. doi: 10.1021/acscatal.5b00192. [DOI] [Google Scholar]
  22. Niu X. Wang K. Bai Y. Du Y. Chen Y. Dong M. Fan W. Selective formation of para-xylene by methanol aromatization over phosphorus-modified ZSM-5 zeolites. Catalyst. 2020;10(5):484. doi: 10.3390/catal10050484. [DOI] [Google Scholar]
  23. Derouane E. G. Dejaifve P. Gabelica Z. Vedrine J. C. Molecular shape selectivity of ZSM-5, modified ZSM-5 and ZSM-11 type zeolites. Faraday Discuss. Chem. Soc. 1981;72:331–344. doi: 10.1039/DC9817200331. [DOI] [Google Scholar]
  24. Zhang X. Han H. Zhang J. Liu B. Song C. Ren L. Zhang A. Guo X. Hierarchical nanosized ZSM-5 for enhanced selectivity of para-xylene in the alkylation of toluene with methanol. ACS Catal. 2025;15(13):11047–11061. doi: 10.1021/acscatal.5c01359. [DOI] [Google Scholar]
  25. Zhang L. Liu N. Dai C. Xu R. Yu G. Chen B. Wang N. Recent advances in shape selectivity of MFI zeolite and its effect on the catalytic performance. Chem. Synth. 2022;3:2. doi: 10.20517/cs.2022.31. [DOI] [Google Scholar]
  26. Jia Y. Wang J. Zhang K. Feng W. Liu S. Ding C. et al., Nanocrystallite self-assembled hierarchical ZSM-5 zeolite microsphere for methanol to aromatics. Microporous Mesoporous Mater. 2017;247:103–115. doi: 10.1016/j.micromeso.2017.03.035. [DOI] [Google Scholar]
  27. Liu M. Cui T. Guo X. Li J. Song C. Stable Zn@ ZSM-5 catalyst via a dry gel conversion process for methanol-to-aromatics reaction. Microporous Mesoporous Mater. 2021;312:110696. doi: 10.1016/j.micromeso.2020.110696. [DOI] [Google Scholar]
  28. Kerstens D. Smeyers B. Van Waeyenberg J. Zhang Q. Yu J. Sels B. F. State of the art and perspectives of hierarchical zeolites: practical overview of synthesis methods and use in catalysis. Adv. Mater. 2020;32:2004690. doi: 10.1002/adma.202004690. [DOI] [PubMed] [Google Scholar]
  29. Cheng C. Li G. Ji D. Zhao Y. Shen J. Regulating hierarchical structure and acidity of HZSM-5 for methanol to aromatics via protective desiliconization and external surface modification. Microporous Mesoporous Mater. 2021;312:110784. doi: 10.1016/j.micromeso.2020.110784. [DOI] [Google Scholar]
  30. Ma Q. Fu T. Li H. Cui L. Li Z. Insight into the Selection of the Post-Treatment Strategy for ZSM-5 Zeolites for the Improvement of Catalytic Stability in the Conversion of Methanol to Hydrocarbons. Ind. Eng. Chem. Res. 2020;59:11125–11138. doi: 10.1021/acs.iecr.0c00084. [DOI] [Google Scholar]
  31. Fang Y. Yang F. He X. Zhu X. Dealumination and desilication for Al-rich HZSM-5 zeolite via steam-alkaline treatment and its application in methanol aromatization. Front. Chem. Sci. Eng. 2019;13:543–553. doi: 10.1007/s11705-018-1778-8. [DOI] [Google Scholar]
  32. Wang J.-X. Cao J.-P. Zhao X.-Y. Liu S.-N. Ren X.-Y. Zhao M. et al., Enhancement of light aromatics from catalytic fast pyrolysis of cellulose over bifunctional hierarchical HZSM-5 modified by hydrogen fluoride and nickel/hydrogen fluoride. Bioresour. Technol. 2019;278:116–123. doi: 10.1016/j.biortech.2019.01.059. [DOI] [PubMed] [Google Scholar]
  33. Yang K. Zhou F. Ma H. Liu C. Ma F. Wu G. Preparation of nanocrystalline ZSM-5 and its catalytic performance in fast pyrolysis of cellulose to produce aromatic hydrocarbons. Microporous Mesoporous Mater. 2022;331:111679. doi: 10.1016/j.micromeso.2022.111679. [DOI] [Google Scholar]
  34. Shestakova D. O. Babina K. A. Sladkovskiy D. A. Parkhomchuk E. V. Seed-assisted synthesis of hierarchical zeolite ZSM-5 in the absence of organic templates. Mater. Chem. Phys. 2022;288:126432. doi: 10.1016/j.matchemphys.2022.126432. [DOI] [Google Scholar]
  35. Alonso-Doncel M. Peral A. Shamzhy M. Čejka J. Sanz R. Serrano D. Untangling the role of the organosilane functional groups in the synthesis of hierarchical ZSM-5 zeolite by crystallization of silanized protozeolitic units. Catal. Today. 2020;345:27–38. doi: 10.1016/j.cattod.2019.11.031. [DOI] [Google Scholar]
  36. Zhao T. Li F. Yu H. Ding S. Li Z. Huang X. et al., Synthesis of mesoporous ZSM-5 zeolites and catalytic cracking of ethanol and oleic acid into light olefins. Appl. Catal., A. 2019;575:101–110. doi: 10.1016/j.apcata.2019.02.011. [DOI] [Google Scholar]
  37. Liu B. Chen Z. Huang J. Chen H. Fang Y. Direct synthesis of hierarchically structured MFI zeolite nanosheet assemblies with tailored activity in benzylation reaction. Microporous Mesoporous Mater. 2019;273:235–242. doi: 10.1016/j.micromeso.2018.07.019. [DOI] [Google Scholar]
  38. Niu X. Sun Y. Lei Z. Qin G. Yang C. Facile synthesis of hierarchical hollow Mn-ZSM-5 zeolite for enhanced cyclohexane catalytic oxidation. Prog. Nat. Sci.:Mater. Int. 2020;30:35–40. doi: 10.1016/j.pnsc.2019.09.006. [DOI] [Google Scholar]
  39. Zhou Z. Jiang R. Chen X. Wang X. Hou H. One-step synthesis of hierarchical lamellar H-ZSM-5 zeolite and catalytic performance of methanol to olefin. J. Solid State Chem. 2021;298:122132. doi: 10.1016/j.jssc.2021.122132. [DOI] [Google Scholar]
  40. Peng S. Yang G. Zhang J. ZSM-5 nanocrystal promoted low-temperature activity of supported manganese oxides for catalytic oxidation of toluene. Inorg. Chem. Commun. 2022;143:109759. doi: 10.1016/j.inoche.2022.109759. [DOI] [Google Scholar]
  41. Liu K. Shoinkhorova T. You X. Gong X. Zhang X. Chung S.-H. et al., The synergistic interplay of hierarchy, crystal size, and Ga-promotion in the methanol-to-aromatics process over ZSM-5 zeolites. Dalton Trans. 2024;53:11344–11353. doi: 10.1039/D4DT00793J. [DOI] [PubMed] [Google Scholar]
  42. Wang Y. Li T. Ouyang Y. Zhong J. Zhang Y. Xiong X. et al., Novel-ordered hierarchical ZSM-5 zeolite with interconnected macro–meso–microporosity for the enhanced methanol to aromatics reaction. Catal. Sci. Technol. 2024;14:2461–2469. doi: 10.1039/D3CY01783D. [DOI] [Google Scholar]
  43. Wei Z. Xia T. Liu M. Cao Q. Xu Y. Zhu K. et al., Alkaline modification of ZSM-5 catalysts for methanol aromatization: The effect of the alkaline concentration. Front. Chem. Sci. Eng. 2015;9:450–460. doi: 10.1007/s11705-015-1542-2. [DOI] [Google Scholar]
  44. Chen L.-H. Sun M.-H. Wang Z. Yang W. Xie Z. Su B.-L. Hierarchically structured zeolites: from design to application. Chem. Rev. 2020;120:11194–11294. doi: 10.1021/acs.chemrev.0c00016. [DOI] [PubMed] [Google Scholar]
  45. Shao J. Fu T. Ma Q. Ma Z. Zhang C. Li Z. Controllable synthesis of nano-ZSM-5 catalysts with large amount and high strength of acid sites for conversion of methanol to hydrocarbons. Microporous Mesoporous Mater. 2019;273:122–132. doi: 10.1016/j.micromeso.2018.07.007. [DOI] [Google Scholar]
  46. Wang K. Ge H. Qin Y. Hollow Zeolites-Confined Isolated (ZnOH)+ Enable High Selectivity and Stability for Methanol to Aromatics. ChemCatChem. 2022;14:e202200022. doi: 10.1002/cctc.202200022. [DOI] [Google Scholar]
  47. Ma Q. Fu T. Ren K. Li H. Jia L. Li Z. Controllable orientation growth of ZSM-5 for methanol to hydrocarbon conversion: cooperative effects of seed induction and medium pH control. Inorg. Chem. 2022;61:13802–13816. doi: 10.1021/acs.inorgchem.2c01628. [DOI] [PubMed] [Google Scholar]
  48. Yue Y. Gu L. Zhou Y. Liu H. Yuan P. Zhu H. et al., Template-free synthesis and catalytic applications of microporous and hierarchical ZSM-5 zeolites from natural aluminosilicate minerals. Ind. Eng. Chem. Res. 2017;56:10069–10077. doi: 10.1021/acs.iecr.7b02531. [DOI] [Google Scholar]
  49. Che Q. Yang M. Wang X. Yang Q. Chen Y. Chen X. et al., Preparation of mesoporous ZSM-5 catalysts using green templates and their performance in biomass catalytic pyrolysis. Bioresour. Technol. 2019;289:121729. doi: 10.1016/j.biortech.2019.121729. [DOI] [PubMed] [Google Scholar]
  50. Tian H. Chen Z. Yang X. Gao P. Jiao C. Zha F. et al., Catalytic performance of methanol to aromatics over hierarchical ZSM-5 zeolite synthesized by a soft template method. Energy Fuels. 2023;37:14180–14191. doi: 10.1021/acs.energyfuels.3c02291. [DOI] [Google Scholar]
  51. Abbasi A. Pourabdollah K. Mokhtarani B. Tailoring hierarchical ZSM-5 with water-soluble polymers templates for BTX production in methanol-to-aromatics. RSC Adv. 2026;16:7040–7055. doi: 10.1039/D5RA08403B. [DOI] [PMC free article] [PubMed] [Google Scholar]
  52. Han J. Chen W. Wang J. Ling L. Zhang Y. Shen X. et al., Insight into dehydrogenation mechanism of methanol to aromatics over GaO+/HZSM-5: Which is the active center, Lewis acid site or Brønsted− Lewis synergistic site? Microporous Mesoporous Mater. 2024;372:113115. doi: 10.1016/j.micromeso.2024.113115. [DOI] [Google Scholar]
  53. Kosinov N. Liu C. Hensen E. J. Pidko E. A. Engineering of transition metal catalysts confined in zeolites. Chem. Mater. 2018;30:3177–3198. doi: 10.1021/acs.chemmater.8b01311. [DOI] [PMC free article] [PubMed] [Google Scholar]
  54. Yang C. Qiu M. Hu S. Chen X. Zeng G. Liu Z. et al., Stable and efficient aromatic yield from methanol over alkali treated hierarchical Zn-containing HZSM-5 zeolites. Microporous Mesoporous Mater. 2016;231:110–116. doi: 10.1016/j.micromeso.2016.05.021. [DOI] [Google Scholar]
  55. Zhang J. Zhu X. Zhang S. Cheng M. Yu M. Wang G. et al., Selective production of para-xylene and light olefins from methanol over the mesostructured Zn–Mg–P/ZSM-5 catalyst. Catal. Sci. Technol. 2019;9:316–326. doi: 10.1039/C8CY02189A. [DOI] [Google Scholar]
  56. Vicente H. Liu C. Gayubo A. G. Castano P. Pidko E. A. Improving the dehydrogenation function and stability of Zn-modified ZSM-5 catalyst in methanol-to-aromatics reaction by Ca addition. Appl. Catal., A. 2024;683:119854. doi: 10.1016/j.apcata.2024.119854. [DOI] [Google Scholar]
  57. Zhu X. Zhang J. Cheng M. Wang G. Yu M. Li C. Methanol aromatization over Mg–P-modified [Zn, Al] ZSM-5 zeolites for efficient coproduction of para-xylene and light olefins. Ind. Eng. Chem. Res. 2019;58:19446–19455. doi: 10.1021/acs.iecr.9b03743. [DOI] [Google Scholar]
  58. Wei Z. Ji Y. Huang Y. Huang J. Huang Y. Yue C. Li J. Tang M. Liu Y. Liu H. Zhu H. Zhu K. Methanol Aromatization over Zn and Ce Modified Hierarchical ZSM-5 Catalysts: Effect of Ce as a Promoter. Adv. Mater. Sci. Eng. 2022;2022:7408284. [Google Scholar]
  59. Zhang X. You X. Wang Y. Zhou H. Zhou X. Chowdhury A. D. The catalytic relevance of hydrothermally substituted, hydrothermally substituted Zn on the zeolite ZSM-5 during the methanol-to-aromatics process. Catal. Sci. Technol. 2025;15(1):185–192. doi: 10.1039/D4CY01168F. [DOI] [Google Scholar]
  60. Wang Y. Li Z. Dai C. Du N. Li T. Wang R. Peng P. Sun H. Zn-P Co-Modified Hierarchical ZSM-5 Zeolites, ZSM-5 Zeolites Directly Synthesized via Dry Gel Conversion for Enhanced Methanol to Aromatics Reaction. Catalysts. 2021;11:1388. doi: 10.3390/catal11111388. [DOI] [Google Scholar]
  61. Xin Y. Qi P. Duan X. Lin H. Yuan Y. Enhanced performance of Zn–Sn/HZSM-5 catalyst for the conversion of methanol to aromatics. Catal. Lett. 2013;143:798–806. doi: 10.1007/s10562-013-1031-5. [DOI] [Google Scholar]
  62. Qiao J. Wang J. Frenkel A. I. Teng J. Chen X. Xiao J. Zhang T. Wang Z. Yuan Z. Yang W. Methanol to aromatics: isolated zinc phosphate groups on HZSM-5 zeolite enhance BTX selectivity and catalytic stability. RSC Adv. 2020;10:5961–5971. doi: 10.1039/C9RA09657D. [DOI] [PMC free article] [PubMed] [Google Scholar]
  63. Lin W. Song Y. Han L. Yang X. Liu J. Peng B. Dehydrogenative aromatization of 1-octene over multifunctional Ni/ZSM-5-P-Fe catalyst. Fuel. 2021;299:120890. doi: 10.1016/j.fuel.2021.120890. [DOI] [Google Scholar]
  64. Zhang Y. Liu Y. Li J. In situ synthesis of metal-containing ZSM-5 and its catalytic performance in aromatization of methanol. ACS Omega. 2022;7:24241–24248. doi: 10.1021/acsomega.2c01442. [DOI] [PMC free article] [PubMed] [Google Scholar]
  65. Jiao C. Jiao Q. Zhang W. Ji Z. Zheng J. Dai W. et al., Synthesis of hierarchical ZSM-5 with ultra-small mesopore structure and its catalytic performance during methanol to hydrocarbons. J. Mater. Sci. 2024;59:16486–16500. doi: 10.1007/s10853-024-10152-2. [DOI] [Google Scholar]
  66. Li B. He Y. Geng R. Shao J. Wei C. Qin Z. Wang J. Fan W. Dong M. Progress on Enhancing The Resistance to Deactivation of Zn-Containing ZSM-5 Catalysts for Light Hydrocarbon Aromatization. ChemCatChem. 2025;17(12):e202500085. doi: 10.1002/cctc.202500085. [DOI] [Google Scholar]
  67. Wang G. Zhang J. Shao J. Sun H. Zuo H. Thermogravimetric analysis of coal char combustion kinetics. J. Iron Steel Res. Int. 2014;21:897–904. doi: 10.1016/S1006-706X(14)60159-X. [DOI] [Google Scholar]
  68. Zhou F. Gao Y. Wu G. Ma F. Liu C. Improved catalytic performance and decreased coke formation in post-treated ZSM-5 zeolites for methanol aromatization. Microporous Mesoporous Mater. 2017;240:96–107. doi: 10.1016/j.micromeso.2016.11.014. [DOI] [Google Scholar]
  69. Luque R. Ahmad A. Tariq S. Mubashir M. Javed M. S. Rajendran S. et al., Functionalized interconnected porous materials for heterogeneous catalysis, energy conversion and storage applications: Recent advances and future perspectives. Mater. Today. 2024;73:105–129. doi: 10.1016/j.mattod.2023.05.001. [DOI] [Google Scholar]
  70. Precisvalle N. Mancinelli M. Ardit M. Beltrami G. Gigli L. Aloise A. Catizzone E. Migliori M. Giordano G. Guidi V. Temperature-Induced Monoclinic-to-Orthorhombic Phase Transition in Protonated ZSM-5 Zeolites with Different Si/Al Ratios: An In-Situ Synchrotron X-ray Powder Diffraction Study. Crystals. 2023;13:979. doi: 10.3390/cryst13060979. [DOI] [Google Scholar]
  71. Jodłowski P. J. Kurowski G. Skoczylas N. Pajdak A. Kudasik M. Jędrzejczyk R. J. et al., Silver and copper modified zeolite imidazole frameworks as sustainable methane storage systems. J. Cleaner Prod. 2022;352:131638. doi: 10.1016/j.jclepro.2022.131638. [DOI] [Google Scholar]
  72. Niu X. Gao J. Wang K. Miao Q. Dong M. Wang G. et al., Influence of crystal size on the catalytic performance of H-ZSM-5 and Zn/H-ZSM-5 in the conversion of methanol to aromatics. Fuel Process. Technol. 2017;157:99–107. doi: 10.1016/j.fuproc.2016.12.006. [DOI] [Google Scholar]
  73. Nezamzadeh-Ejhieh A. Shams-Ghahfarokhi Z. Photodegradation of Methyl Green by Nickel-Dimethylglyoxime/ZSM-5 zeolite as a heterogeneous catalyst. J. Chem. 2013;2013:104093. doi: 10.1155/2013/104093. [DOI] [Google Scholar]
  74. Niu X. Li J. Zhang L. Lei Z. Zhao X. Yang C. ZSM-5 functionalized in situ with manganese ions for the catalytic oxidation of cyclohexane. RSC Adv. 2017;7:50619–50625. doi: 10.1039/C7RA10771D. [DOI] [Google Scholar]
  75. Wei Z. Chen L. Cao Q. Wen Z. Zhou Z. Xu Y. et al., Steamed Zn/ZSM-5 catalysts for improved methanol aromatization with high stability. Fuel Process. Technol. 2017;162:66–77. doi: 10.1016/j.fuproc.2017.03.026. [DOI] [Google Scholar]
  76. Niu X. Gao J. Wang K. Miao Q. Dong M. Wang G. et al., Influence of crystal size on the catalytic performance of H-ZSM-5 and Zn/H-ZSM-5 in the conversion of methanol to aromatics. Fuel Process. Technol. 2017;157:99–107. doi: 10.1016/j.fuproc.2016.12.006. [DOI] [Google Scholar]
  77. Niu X. Gao J. Miao Q. Dong M. Wang G. Fan W. et al., Influence of preparation method on the performance of Zn-containing HZSM-5 catalysts in methanol-to-aromatics. Microporous Mesoporous Mater. 2014;197:252–261. doi: 10.1016/j.micromeso.2014.06.027. [DOI] [Google Scholar]
  78. Pan T. Ge S. Yu M. Ju Y. Zhang R. Wu P. et al., Synthesis and consequence of Zn modified ZSM-5 zeolite supported Ni catalyst for catalytic aromatization of olefin/paraffin. Fuel. 2022;311:122629. doi: 10.1016/j.fuel.2021.122629. [DOI] [Google Scholar]
  79. Zhang L. Gao W. Wang F. Wang C. Liang J. Guo X. et al., Highly selective synthesis of light aromatics from CO2 by chromium-doped ZrO2 aerogels in tandem with HZSM-5@ SiO2 catalyst. Appl. Catal., B. 2023;328:122535. doi: 10.1016/j.apcatb.2023.122535. [DOI] [Google Scholar]
  80. Khatrin I. Kusuma R. H. Kadja G. T. M. Krisnandi Y. K. Significance of ZSM-5 hierarchical structure on catalytic cracking: Intra-vs inter-crystalline mesoporosity. Inorg. Chem. Commun. 2023;149:110447. doi: 10.1016/j.inoche.2023.110447. [DOI] [Google Scholar]
  81. Xue Y. Cui X. Shan J. Gao S. Wang S. Zheng H. et al., Tailoring porosity and acidity of Sn-modified ZSM-5 for co-aromatization of methanol with 2-methylfuran. Fuel. 2023;340:127440. doi: 10.1016/j.fuel.2023.127440. [DOI] [Google Scholar]
  82. Zhan J. Wang Y. He T. Sheng L. Wu B. Liu Q. et al., Nonionic polymer and amino acid-assisted synthesis of ZSM-5 nanocrystals and their catalytic application in the alkylation of 2-methylnaphthalene. Dalton Trans. 2024;53:7384–7396. doi: 10.1039/D4DT00096J. [DOI] [PubMed] [Google Scholar]
  83. Biriaei R. Nohair B. Kaliaguine S. A facile route to synthesize mesoporous ZSM-5 with hexagonal arrays using P123 triblock copolymer. Microporous Mesoporous Mater. 2020;298:110067. doi: 10.1016/j.micromeso.2020.110067. [DOI] [Google Scholar]
  84. Anekwe I. M. S. Oboirien B. Isa Y. M. Effects of transition metal doping on the properties and catalytic performance of ZSM-5 zeolite catalyst on ethanol-to-hydrocarbons conversion. Fuel Commun. 2024;18:100101. doi: 10.1016/j.jfueco.2023.100101. [DOI] [Google Scholar]
  85. Peng H. Wang A. He P. Harrhy J. Meng S. Song H. Solvent-free catalytic conversion of xylose with methane to aromatics over Zn-Cr modified zeolite catalyst. Fuel. 2019;253:988–996. doi: 10.1016/j.fuel.2019.05.088. [DOI] [Google Scholar]
  86. Saini S. Oluokun T. Sharma B. Verma A. Vorontsov A. Smirniotis P. G. et al., Cr-and Ga-Modified ZSM-5 Catalyst for the Production of Renewable BTX from Bioethanol. ChemPlusChem. 2024;89:e202300572. doi: 10.1002/cplu.202300572. [DOI] [PubMed] [Google Scholar]
  87. Jin W. Qiao J. Yu J. Wang Y. Cao J. Influence of hollow ZSM-5 zeolites prepared by treatment with different alkalis on the catalytic conversion of methanol to aromatics. Energy Fuels. 2020;34:14633–14646. doi: 10.1021/acs.energyfuels.0c02345. [DOI] [Google Scholar]
  88. Ahmed R. Sinnathambi C. Subbarao D. Kinetics of de-coking of spent reforming catalyst. J. Appl. Sci. 2011;11:1225–1230. doi: 10.3923/jas.2011.1225.1230. [DOI] [Google Scholar]
  89. Silva B. J. Sousa L. V. Sarmento L. R. Melo A. C. Silva D. S. Quintela P. H. Alencar S. L. Silva A. O. Effect of coke deposition over microporous and hierarchical ZSM-23 zeolite. J. Therm. Anal. Calorim. 2022;147:3161–3170. doi: 10.1007/s10973-021-10740-3. [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Data Availability Statement

The data supporting this article are available within the published article.


Articles from RSC Advances are provided here courtesy of Royal Society of Chemistry

RESOURCES