Abstract
Cariogenic biofilms primarily associated with Streptococcus mutans and Lactobacillus acidophilus contribute to one of the most prevalent chronic oral diseases worldwide. Although current Casein Phosphopeptide-Amorphous Calcium Phosphate (CPP-ACP) systems are effective in remineralization, they lack direct biofilm-disrupting capabilities, highlighting the need for multifunctional materials. A biogenic Ag-HAp-MSN nanocomposite, previously synthesized using Cissus quadrangularis extract and confirmed to possess favourable physicochemical properties and cytocompatibility, was evaluated for its antibacterial and anti-biofilm efficacy. Antibacterial activity was assessed using agar well diffusion, Minimum Inhibitory Concentration (MIC), and Minimum Bactericidal Concentration (MBC) assays, while anti-biofilm activity was analysed via crystal violet inhibition, acridine orange/ethidium bromide (AO/EB) live-dead fluorescence, and Confocal Laser Scanning Microscopy (CLSM). GC Tooth Mousse served as a contextual clinical reference. At 1000 µg/mL, the nanocomposite produced ZOI values of 25 mm (S. mutans) and 29 mm (L. acidophilus), outperforming all individual components. The MIC values were 250 µg/mL (S. mutans) and 125 µg/mL (L. acidophilus), representing a 2–4-fold improvement, with MBC/MIC ratios of 2, confirming bactericidal action. Crystal violet biofilm inhibition reached 82.53% and 87.53%, while AO/EB dead-cell fractions were 83.63% and 89.33%, respectively (p < 0.001 vs. all controls). Under agar diffusion conditions, the nanocomposite showed inhibition zones comparable to GC Tooth Mousse against L. acidophilus at 800 µg/mL. These findings support further investigation of biogenic Ag-HAp-MSN nanocomposite for anti-cariogenic applications.
Keywords: Ag-HAp-MSN, Anti-biofilm, Biogenic Nanocomposite, Cissus quadrangularis, CPP-ACP, Dental caries, Streptococcus mutans, Lactobacillus acidophilus
Introduction
Dental caries is one of the most prevalent chronic oral diseases worldwide. Early colonisation of the enamel surface by Streptococcus mutans sets in motion an acidic microenvironment that progressively marginalises competing flora; the sustained fermentative activity of both S. mutans and Lactobacillus acidophilus drives hard-tissue demineralisation [1, 2]. Each organism tolerates and generates acid, and their combined contribution to caries initiation and progression is well established [2–4]. Current chemoprevention strategies centre on fluoride and CPP-ACP formulations, with GC Tooth Mousse representing the most widely adopted non-fluoride CPP-ACP option [5–7]. Although, these agents effectively support remineralisation, they are not primarily designed to disrupt cariogenic biofilms, and their clinical value is limited by strict adherence to use regimens. Therefore, there is an unmet need for materials capable of both biofilm disruption and remineralisation promotion. Nanoparticle-based approaches have attracted increasing attention for this problem. Silver nanoparticles are bactericidal via at least three independent routes: membrane rupture, reactive oxygen species (ROS) induction, and enzyme/DNA interference [8–11] and the simultaneous action of these pathways make resistance emergence less likely than with single-target antibiotics. Nanohydroxyapatite (n-HAp) has a mineral composition that is near-identical to that of enamel, and its remineralisation and biocompatibility credentials are well established [12–14].
Mesoporous silica nanoparticles (MSNs) offer their architectural utility through large surface area and tunable mesopore diameter, enabling sustained, site-directed ion release [15–17]. In green synthesis, plant phytoconstituents can simultaneously reduce silver ions, cap particle surfaces, and provide functionalisation in a single step, enabling a safer multifunctional anti-cariogenic platform without harmful reducing agents [18–20]. Cissus quadrangularis (CQ) was selected as the biogenic mediator for pertinent reasons. It has been proven to have potential as a reducing agent in the synthesis of AgNP [21–23]. Its phytochemicals (phenolic, terpenoid, and saponin) also provide antioxidant and anti-inflammatory effects to the final particles [24, 25]. The analysis of total phenolic content showed that Cissus quadrangularis extract had a phytochemical yield of 88.9 mg GAE/g dry weight. The major strength of biogenic synthesis is that phytoconstituents do not merely act as reducing agents; they also remain associated with the nanoparticle surface and may contribute to additional functional benefits. After synthesis, these phytocompounds bind to the particle surface, forming an organic corona, which is crucial for drug formulation because it can alter the surface charge, retard aggregation of particles in protein-rich media, and form hydrogen bonds with mucosal glycoproteins. Other advantages include residual antioxidant activity at the application site, which cannot be provided by sodium borohydride and other conventional reducing agents [26].
Component-level research has also been conducted: Ag-HAp composites [27] and dental AgNP formulations [28] have been defined; MSN carriers have been studied in terms of dental adhesive loading [29] and controlled release [30] and nano-HAp has clinical evidence in a variety of dental applications [31]. We previously reported the phytosynthesis, physicochemical characterisation, and cytocompatibility assessment of a tripartite Ag-HAp-MSN nanocomposite comprising Cissus quadrangularis aqueous extract [32]. However, its antimicrobial properties have not yet been explored. This study builds on the existing literature by conducting a systematic study of antibacterial and anti-biofilm activity against S. mutans and L. acidophilus in the presence of GC Tooth Mousse as an exemplary clinical source in the ZOI test. To our knowledge, this is the first study to integrate antibacterial, anti-biofilm, and CLSM depth-penetration analysis in a biogenic Ag-HAp-MSN system for anti-cariogenic applications. The panel consisted of five assays, including bacteriostatic, bactericidal, and anti-biofilm endpoints, with CLSM 3D Z-stack imaging as a supplement. Prior to conducting biological assays, the primary physicochemical properties of the current synthesis batch were re-evaluated to ensure consistency with the previously documented material [32].
Materials and methods
Plant material and extract preparation
Fresh stems of Cissus quadrangularis were commercially procured from certified organic farms in and around Chennai (12.97°N, 80.22°E) and Kancheepuram (12.83°N, 79.70°E), Tamil Nadu, India, where the plant is widely cultivated and commercially available. The plant material was authenticated by the School of Life Sciences, SRM Institute of Science and Technology (SRMIST), Kattankulathur, Tamil Nadu, India (Authentication Ref: SRM-BOT-2024-12). Since the plant material was commercially procured and not collected from protected wild populations, no special collection permits or licences were required. All procurement and use complied with applicable local and national guidelines of India. The authenticated stem material was extracted using a Soxhlet apparatus (50 g powdered material in 150 mL distilled water at approximately 90 °C for 48 h) as previously reported [32]. The filtrate was stored at 4 °C until further use. Phytochemical yield (total phenolic content) was 88.9 mg GAE/g dry weight, consistent with our previous report [32].
Nanoparticle synthesis
Silver nanoparticles (AgNPs)
To prepare AgNPs, Cissus quadrangularis extract (20 mL) was mixed with 50 mM AgNO3 (80 mL) and stirred at 60 °C, 450 rpm for 6 h [32]. The gradual change in colour from light yellow to deep brown was used to confirm Ag+ reduction and the formation of particles. The synthesized AgNPs were centrifugally washed and lyophilized.
Mesoporous silica nanoparticles (MSNs)
MSN was prepared using a CTAB template via sol-gel synthesis [32]. NaOH was added to the CTAB solution to a pH of 11 and TEOS dropped on the mixture under constant stirring to promote silica condensation. The blend was allowed to age overnight at room temperature. The solution with MSN was filtered, washed thoroughly, and then calcined at 55 °C in 5 h. The surfactant was removed by this process, and mesopore channels characteristic of MSNs were revealed.
Nanohydroxyapatite (n-HAp)
Biogenic n-HAp was synthesized via a modified precipitation method as previously described [32]. Briefly, 80 mL of 0.1 mol/L CaCl2 was reacted with 20 mL of Cissus quadrangularis extract (100 mg/mL) for 3 h, followed by drop-wise addition of 60 mL of 0.1 mol/L Na2HPO4 12H2O. The reaction was maintained at pH 9.0 and 60 °C for 2 h. The resulting precipitate was aged overnight, centrifuged (3000 rpm for 30 min) and freeze-dried at − 40 °C for 48 h.
Tripartite Ag-HAp-MSN nanocomposite
The composite was assembled by a one-pot synthesis [32]. AgNPs and n-HAp (1:1 w/w) were dispersed in water; TEOS and CTAB were added to drive MSN shell formation around the pre-formed cores at pH 10, overnight. Products were calcined, washed, freeze-dried, and sealed in vials.
Physicochemical characterisation
Physicochemical characterisation of all four materials — AgNPs, n-HAp, MSNs, and the Ag-HAp-MSN nanocomposite — was performed using UV-Vis spectroscopy (200–800 nm), XRD (Cu-Kα, 2θ 10–80)0, Scherrer equation), FTIR (400–4000 cm⁻¹), DLS and zeta potential (Malvern Zetasizer Nano ZS), BET/BJH analysis (N₂ isotherms at 77.35 K, Quantachrome Autosorb iQ), and TEM-SAED (carbon-coated copper grids). Key parameters were reconfirmed in the present batch prior to biological evaluation to verify reproducibility of the synthesis.
Antibacterial and anti-biofilm assays
Zone of inhibition (ZOI), Minimum Inhibitory Concentration (MIC), Minimum Bactericidal Concentration (MBC), and crystal violet biofilm biomass quantification were performed at Simbioen Labs and Scientific Services Private Limited (Sample code: SBTW/13/12/020, Chennai, India). CLSM 3D Z-stack imaging was performed independently at Saveetha Dental College and Hospital, SIMATS, Chennai, on identically prepared and treated biofilm samples. AO/EB fluorescence quantification was performed at Simbioen Labs on a separate parallel set of biofilm samples using an inverted epifluorescence microscope. All assays were performed in triplicates.
Bacterial strains, culture conditions, and inoculum verification
S. mutans (MTCC 890) and L. acidophilus (MTCC 10307) were procured from the Institute of Microbial Technology (Chandigarh, India). S. mutans was maintained on Brain Heart Infusion (BHI) agar at 37 °C under anaerobic conditions for 24 h; L. acidophilus on MRS agar under microaerophilic conditions for 48 h. The working inocula were adjusted to the 0.5 McFarland standard (~ 1 × 10⁸ CFU/mL). Prior to each test, the inoculum density was validated using serial dilution plating (10⁻⁴ to 10⁻⁷ dilutions). All experimental runs confirmed viable counts of ≥ 1 × 10⁸ CFU/mL. Supplementary file with Fig. S1 shows representative streak plates.
Zone of inhibition (ZOI)
ZOI was measured using the agar well diffusion method following the Clinical and Laboratory Standards Institute (CLSI) guidelines. Mueller-Hinton agar was surface-inoculated with 1 × 10⁸ CFU/mL suspensions; 8 mm wells were punched with a sterile cork borer and each received 50 µL of test material at 1000, 500, 250, or 100 µg/mL. Erythromycin: Penicillin (1:1, 10 µg) served as the positive control to confirm assay sensitivity; DMSO (equivalent volume) served as the negative control. The plates were incubated at 37 °C for 24 h. The inhibition zone diameters were independently measured by two observers to the nearest millimetre and the means recorded.
GC tooth mousse contextual ZOI reference
GC Tooth Mousse (CPP-ACP cream, GC Corporation, Japan) was included as a contextual clinical reference in a separate ZOI experiment conducted at Saveetha Dental College. Each well received 50 µL of GC Tooth Mousse cream. The quantities of 20 µg/well and 40 µg/well refer to the total mass of cream dispensed; for comparative purposes these are treated as equivalent to 400 µg/mL and 800 µg/mL of nanocomposite suspension respectively. This comparison was based on the total dispensed mass rather than the active CPP-ACP constituent concentration, which should be considered when interpreting the ZOI equivalence data. MIC/MBC was not determined for GC Tooth Mousse because its viscous cream formulation is incompatible with the broth microdilution methodology; therefore, it is presented as a contextual reference only.
MIC and MBC determination
For MIC determination, we used broth microdilution in 96-well polypropylene plates, following CLSI M07 guidelines. Dilutions of 2 folds were done in BHI broth, and the concentrations ranged from 1000 –7.81 µg/mL. All wells were inoculated with 5 × 105 CFU/mL and incubated at 37 °C. The lowest concentration was used to define the MIC and OD₆₂₀ was used to confirm clarity. The MBC was assessed by inoculating freshly prepared BHI agar plates with contents of all of the clear wells. The lowest culture concentration at which no colonies were produced, was considered the MBC, representing a kill rate of 99.9% relative to the initial inoculum. The percentage growth inhibition at each dilution rate was determined relative to the untreated growth control.
Anti-biofilm assay (crystal violet biomass)
The anti-biofilm property of the nanocomposite was tested using a constant crystal violet biomass test in a prevention model setup. Bacterial cultures that had been grown overnight were diluted to OD₆₀₀ 0.05 in BHI broth and transferred to flat-bottomed 96- well plates. It is worth noting that nanocomposites were introduced into MBC, simultaneously with the inoculum, which indicates that these results are indicative of biofilm growth inhibition, rather than degradation of an existing film. After incubation, the planktonic fraction was aspirated and the remaining biofilm was washed once with Phosphate-Buffered Saline (PBS). Crystal violet (0.1% w/v) was applied for 5 min, excess was removed with PBS, and the plates were air-dried. The dye was solubilised in 100 µL of 33% glacial acetic acid, and absorbance was measured at 595 nm. The results are expressed as percentage reduction in the biomass relative to that of the untreated control.
CLSM Z-stack 3D imaging (qualitative)
CLSM was performed at Saveetha Dental College on biofilms grown for 24 h, followed by exposure to nanocomposite at MBC for a further 24 h in glass-bottom confocal dishes. Z-stack reconstruction across the full biofilm depth, mapped the live (green fluorescence) and dead (red fluorescence) bacterial populations in three dimensions, for both S. mutans and L. acidophilus. Three-dimensional reconstructions and 2D cross-sections were acquired to visualise biofilm thickness, structural integrity, and depth of bactericidal penetration.
AO/EB fluorescence live/dead quantification
Quantitative live/dead assessment was performed at Simbioen Labs using a parallel set of biofilm samples prepared and treated under identical conditions. Biofilms were stained with acridine orange (AO) and ethidium bromide (EB) (100 mg/L each) in the dark, rinsed with PBS, and examined under an inverted epifluorescence microscope. Viable cells produced green fluorescence (AO); membrane-compromised cells produced red fluorescence (EB). The dead cell fractions were measured in three randomly selected fields per sample using ImageJ. The untreated control (> 88% viable) served as a 100% viability reference.
Statistical analysis
The results are presented as mean ± SD from three independent experimental runs. One-way ANOVA followed by Tukey’s post-hoc test was used for inter-group comparisons. A p-value < 0.05 was considered statistically significant. Unless otherwise specified, intergroup comparisons showed statistical significance with p < 0.001.
Results
Physicochemical characterisation
UV-Vis spectroscopy
The obtained UV-Vis spectra were consistent with the previous findings [32]. AgNPs exhibited a peak at 450 nm, which was attributed to the characteristic SPR of silver nanoparticles [9]. n-HAp showed a broad phosphate band at 310 nm [13], whereas MSNs exhibited a monotonically decreasing featureless absorption profile between 200 and 350 nm [18]. The SPR peak of nanocomposite shifted to around 490 nm, reflecting a 40 nm red shift, implying strong electronic interactions within the tripartite structure [27] (Fig. 1).
Fig. 1.

UV-Vis absorption spectra: (a) AgNPs (SPR peak 450 nm), (b) n-HAp (broad band 310 nm), (c) MSNs (gradual decline 200–350 nm), (d) Ag-HAp-MSN nanocomposite (combined peaks 310 & 490 nm), confirming successful synthesis and tripartite integration
X-ray diffraction (XRD)
XRD confirmed that all four materials were phase identical with the composite diffractogram being consistent with previously reported data [32]. The composite exhibited a mixture of Face-Centred Cubic (FCC) silver (JCPDS 04-0783), and hexagonal HAp (JCPDS 09-0432) with no new peaks appearing, indicating that the tripartite assembly did not lose phase integrity. At approximately 22°, the characteristic amorphous silica peak of MSNs was observed. The size of Scherrer crystallites, or the average size of the coherent domains within each particle, calculated using the Scherrer equation [33], was 165 nm in AgNPs, 152 nm in n-HAp, 86 nm in MSNs and 169 nm in the composite (Fig. 2). However, the values are outside the traditional primary nanoparticle size and match those of the literature [32]. The DLS hydrodynamic diameters (Table 1) were significantly larger, indicating that the particles have aggregated with each other and that the CQ phytochemical organic shell, covered the particle surfaces [22].
Fig. 2.

XRD diffractograms of AgNPs, n-HAp, MSNs, and Ag-HAp-MSN nanocomposite confirming the crystalline phases: FCC silver peaks (38.5°, 44.8°), hexagonal n-HAp reflections, and the amorphous MSN hump at ~ 22°
Table 1.
Physicochemical characterisation summary of synthesised nanoparticles
| Sample | UV-Vis (nm) | XRD Size (nm) | FTIR Key Bands (cm⁻¹) | Zeta (mV) | BET (m²/g) |
|---|---|---|---|---|---|
| AgNPs | 450 | 165 | 1747 (C = O); 3583, 3672 (O-H); CQ capping confirmed | −34.7 | N/A¹ |
| n-HAp | 310 | 152 | 1016 (P-O phosphate) | + 10.2 | N/A¹ |
| MSNs | 200–350 | 86 | ~ 1080 (Si-O-Si); ~960 (Si-OH); ~1641 (H₂O bend) | −7.28 | N/A¹ |
| Ag-HAp-MSN | 310 & 490 | 169 | 1012–1091; ~960; ~490 (novel Ag–O²); ~1641; 1747 | −9.22 | 108.0 |
¹N/A = not applicable; BET was performed on the final composite only, as the intent was to verify intact mesopore architecture after tripartite assembly. ²Novel band at ~ 490 cm⁻¹ assigned to Ag–O stretching (see Sect. 3.1.3)
FTIR spectroscopy
The FTIR spectra aligned with previously reported findings [32]. The AgNP spectra exhibited a C = O band at 1747 cm⁻¹ and two O–H stretching bands at 3583 and 3672 cm⁻¹, therefore affirming the existence of CQ-derived phytoconstituent capping. The n-HAp spectra exhibited a distinctive phosphate band at 1016 cm⁻¹. MSNs displayed Si–O–Si asymmetric stretching at around 1080 cm⁻¹, Si–OH silanol groups at around 960 cm⁻¹, and an adsorbed water bending mode at about 1641 cm⁻¹. All principal component bands were preserved in the nanocomposite. An extra band emerged at around 490 cm⁻¹, which was not present in any of the individual components and may correspond to Ag–O stretching. This band suggests possible inter-component interactions within the composite matrix. Comparable vibrational modes within the 420–520 cm⁻¹ range have been reported in the silver–silica systems [34], supporting this classification. This coordination trait indicates the structural incorporation of silver into the HAp–MSN system, perhaps enhancing stability and regulating ion release (Fig. 3).
Fig. 3.

FTIR spectra of AgNPs, n-HAp, MSNs, and Ag-HAp-MSN nanocomposite. A novel band at ~ 490 cm⁻¹, present exclusively in the composite (arrowed), may correspond to Ag–O stretching, suggesting interaction between the components within the composite structure
Zeta potential and particle size (DLS)
Zeta potential values: AgNPs − 34.7 mV (high stability attributed to CQ phytochemical corona), MSNs − 7.28 mV, n-HAp + 10.2 mV. The net zeta potential of the tripartite integration was − 9.22 mV, indicating charge compensation among the component surfaces. This value is below the conventional ± 30 mV threshold for electrostatic stability; therefore, additional surface stabilisation strategies may be required prior to in vivo assessment. The physicochemical data are consolidated in Table 1; Fig. 4.
Fig. 4.

Zeta potential distribution and DLS hydrodynamic size of AgNPs, MSNs, n-HAp, and Ag-HAp-MSN nanocomposite. Composite zeta potential: −9.22 mV
BET surface area analysis
The N₂ adsorption–desorption isotherm of the final composite (Fig. 5) exhibited a Type IV profile with H1 hysteresis, clearly indicating the presence of ordered cylindrical mesopores [17]. The BET surface area was 108.0 m²/g, the total pore volume was 0.2847 cm³/g, and the mean pore diameter was 10.68 nm. Collectively, these findings indicate that the MSN mesopore structure retained its structural integrity during the tripartite assembly and calcination processes. BET analysis was conducted only on the composite to ascertain that the mesopore architecture remained intact after the synthesis procedure.
Fig. 5.

N2 adsorption–desorption isotherm of Ag-HAp-MSN nanocomposite showing type IV mesoporous profile. BET surface area = 108.0 m2/g;total pore volume = 0.2847 cm3/g; mean pore diameter = 10.68 nm
TEM and SAED analysis
Representative TEM images (Fig. 6) confirmed the characteristic morphology of the synthesized materials. AgNPs exhibited predominantly spherical to quasi-spherical particles with mild agglomeration, n-HAp displayed characteristic needle-to-rod-shaped morphology, MSNs exhibited predominantly spherical morphology with relatively uniform particle distribution, and the Ag-HAp-MSN nanocomposite showed heterogeneous multi-component aggregates, demonstrating successful integration of the constituent materials. The corresponding SAED patterns (Fig. 7) further supported the structural characteristics of the synthesized materials, with diffraction features consistent with the crystalline nature of AgNPs, n-HAp, and the Ag-HAp-MSN nanocomposite, while the MSN SAED pattern exhibited the diffuse diffraction characteristics expected for mesoporous silica.
Fig. 6.

Representative transmission electron microscopy (TEM) images of the synthesized nanomaterials and Ag-HAp-MSN nanocomposite acquired at different magnifications (scale bars are indicated in each panel). A–B Silver nanoparticles (AgNPs) exhibiting predominantly spherical to quasi-spherical morphology with mild agglomeration. C–D Nanohydroxyapatite (n-HAp) showing characteristic needle-to-rod-shaped morphology. E–F Mesoporous silica nanoparticles (MSNs) displaying predominantly spherical morphology with relatively uniform particle distribution. G–H Ag-HAp-MSN nanocomposite demonstrating heterogeneous multi-component aggregates, confirming the successful integration of AgNPs, n-HAp, and MSNs into a composite structure
Fig. 7.

Selected area electron diffraction (SAED) patterns of the synthesized nanomaterials. A AgNPs, (B) n-HAp, (C) MSNs, and (D) Ag-HAp-MSN nanocomposite. The SAED patterns corroborate the structural characteristics of the synthesized materials and complement the TEM morphological observations presented in Fig. 6
Zone of inhibition (ZOI)
ZOI data are in Table 2. The nanocomposite produced the largest zones at every concentration: 25.00 ± 0.58 mm (S. mutans) and 29.00 ± 0.58 mm (L. acidophilus) at 1000 µg/mL, outperforming AgNPs, MSNs, and n-HAp individually at all doses. The activity was dose-dependent across all materials. n-HAp showed no measurable zone at 100 µg/mL against either organism. DMSO produced no zone. The inhibition zone diameters presented in Table 2 represent direct measurements obtained from the agar plates immediately after incubation, while the corresponding photographs in Fig. 8 are representative images illustrating the assay.
Table 2.
Mean zone of inhibition (ZOI, mm) measured directly on agar plates against cariogenic pathogens (Mean ± SD, n = 3)
| Sample | SM 1000 | SM 500 | SM 250 | SM 100 | LA 1000 | LA 500 | LA 250 | LA 100 |
|---|---|---|---|---|---|---|---|---|
| Ag-HAp-MSN | 25.00 ± 0.58 | 22.00 ± 0.45 | 18.00 ± 0.32 | 16.00 ± 0.32 | 29.00 ± 0.58 | 25.00 ± 0.41 | 23.00 ± 0.47 | 21.00 ± 0.47 |
| AgNPs | 24.00 ± 0.41 | 19.00 ± 0.38 | 16.00 ± 0.28 | 15.00 ± 0.28 | 28.00 ± 0.55 | 24.00 ± 0.35 | 22.00 ± 0.35 | 20.00 ± 0.31 |
| MSNs | 22.00 ± 0.20 | 19.00 ± 0.25 | 17.00 ± 0.21 | 13.00 ± 0.18 | 23.00 ± 0.24 | 20.00 ± 0.22 | 16.00 ± 0.22 | 14.00 ± 0.22 |
| n-HAp | 20.00 ± 0.37 | 17.00 ± 0.29 | 14.00 ± 0.25 | * | 21.00 ± 0.35 | 18.00 ± 0.31 | 15.00 ± 0.25 | * |
| DMSO (neg. ctrl) | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 |
ZOI in mm at all four concentrations (1000, 500, 250, 100 µg/mL) for both organisms. SM = S. mutans; LA = L. acidophilus. * = no zone of inhibition detected at 100 µg/mL. Mean ± SD (n = 3). Agar well diffusion, CLSI guidelines; 8 mm wells, 50 µL per well
Fig. 8.

Representative agar well diffusion assay showing the antibacterial activity of the Ag-HAp-MSN nanocomposite against (a) S. mutans and (b) L. acidophilus at 1000, 500, 250, and 100 µg/mL concentrations. Zone of inhibition (ZOI) diameters reported in Table 2 were measured directly on the agar plates immediately after incubation; the photographs are representative images provided for qualitative illustration of the assay (n = 3 independent experiments)
GC tooth mousse contextual ZOI reference
Wells received 50 µL; thus, 20 µg/well = 400 µg/mL and 40 µg/well = 800 µg/mL. At 800 µg/mL, the nanocomposite produced a ZOI of 12.00 ± 0.16 mm against S. mutans and 15.00 ± 0.16 mm against L. acidophilus; the latter was statistically comparable to GC Tooth Mousse (15.00 ± 0.13 mm; p > 0.05). At 400 µg/mL, the nanocomposite produced smaller zones than GC Tooth Mousse against both organisms. Against S. mutans, GC Tooth Mousse showed greater activity at both doses, consistent with the documented tolerance of this species to non-antibiotic agents. The representative plates are shown in Table 3; Fig. 9.
Table 3.
Comparative ZOI (mm) — Ag-HAp-MSN vs. GC tooth mousse (Mean ± SD, n = 3)
| Sample (dose) | SM ZOI (mm) | LA ZOI (mm) | Equiv. conc. | vs. SM p | vs. LA p |
|---|---|---|---|---|---|
| DMSO (neg. ctrl) | 0 | 0 | N/A | — | — |
| Erythromycin: Penicillin (10 µg, pos. ctrl) | 17.00 ± 0.13 | 18.00 ± 0.15 | N/A | — | — |
| GC Tooth Mousse (20 µg) | 15.00 ± 0.09 | 15.00 ± 0.13 | 400 µg/mL | — | — |
| GC Tooth Mousse (40 µg) | 15.00 ± 0.11 | 15.00 ± 0.13 | 800 µg/mL | — | — |
| Ag-HAp-MSN (20 µg) | 11.00 ± 0.11 | 13.00 ± 0.21 | 400 µg/mL | < 0.05 | < 0.05 |
| Ag-HAp-MSN (40 µg) | 12.00 ± 0.16 | 15.00 ± 0.16 | 800 µg/mL | < 0.05 | > 0.05 |
SM = S. mutans; LA = L. acidophilus. Well volume 50 µL throughout; dose/well converted to µg/mL as shown. p-values: nanocomposite vs. GC Tooth Mousse, one-way ANOVA with Tukey’s post-hoc
Fig. 9.

Comparative ZOI plates (contextual reference): Ag-HAp-MSN nanocomposite vs. GC Tooth Mousse against (a) S. mutans and (b) L. acidophilus (n = 3; representative plates shown). Well key: A = DMSO (neg. ctrl, 0 mm); B = Erythromycin: Penicillin 1:1 (10 µg, pos. ctrl); C = GC Tooth Mousse (20 µg/well, 400 µg/mL); D = Ag-HAp-MSN (20 µg/well); E = Ag-HAp-MSN (40 µg/well, 800 µg/mL)
MIC and MBC
The MIC and MBC values are presented in Table 4 and the percentage inhibition data are presented in Tables 5 and 6. The nanocomposite achieved the lowest MIC and MBC values among all tested materials against both organisms. MIC was 250 µg/mL (S. mutans) and 125 µg/mL (L. acidophilus), a 2–4-fold improvement over individual components. All four materials showed MBC/MIC = 2, satisfying the bactericidal classification threshold of ≤ 4. The composite exceeded 93% growth inhibition of S. mutans and 95% of L. acidophilus at 1000 µg/mL. Optical density-based percentage inhibition curves validated dose-dependent suppression over the whole range of 1000–7.81 µg/mL (Fig. 10). The MBC assessment verified the absence of detectable colonies at the specified bactericidal concentrations for all compounds.
Table 4.
MIC and MBC values (µg/mL)
| Sample | SM MIC | SM MBC | LA MIC | LA MBC |
|---|---|---|---|---|
| Ag-HAp-MSN | 250 | 500 | 125 | 250 |
| AgNPs | 500 | 1000 | 250 | 500 |
| MSNs | 500 | 1000 | 250 | 500 |
| n-HAp | 500 | 1000 | 500 | 1000 |
SM = S. mutans; LA = L. acidophilus. All MBC/MIC ratios = 2 (≤ 4 bactericidal criterion). Broth microdilution, CLSI M07
Table 5.
Percentage growth inhibition of S. mutans (Mean ± SD, n = 3)
| Conc. (µg/mL) | Composite | AgNPs | MSNs | n-HAp |
|---|---|---|---|---|
| 1000 | 93.32 ± 0.57 | 90.78 ± 0.53 | 89.51 ± 0.41 | 86.52 ± 0.54 |
| 500 | 89.50 ± 0.28 | 85.15 ± 0.72 | 81.52 ± 0.12 | 80.10 ± 0.18 |
| 250 | 82.18 ± 0.52 | 78.20 ± 0.34 | 75.86 ± 0.35 | 71.66 ± 0.28 |
| 125 | 75.04 ± 0.62 | 70.80 ± 1.01 | 66.61 ± 0.23 | 60.50 ± 0.20 |
| 62.5 | 66.43 ± 0.84 | 61.25 ± 0.17 | 54.87 ± 0.38 | 48.25 ± 0.46 |
| 31.25 | 54.33 ± 1.23 | 49.56 ± 0.12 | 41.76 ± 0.45 | 39.77 ± 0.13 |
| 15.62 | 41.81 ± 0.46 | 32.40 ± 0.37 | 32.50 ± 0.30 | 30.05 ± 0.21 |
| 7.81 | 28.89 ± 0.30 | 26.81 ± 0.15 | 21.42 ± 0.34 | 19.49 ± 0.37 |
Table 6.
Percentage growth inhibition of L. acidophilus (Mean ± SD, n = 3)
| Conc. (µg/mL) | Composite | AgNPs | MSNs | n-HAp |
|---|---|---|---|---|
| 1000 | 95.33 ± 0.19 | 94.33 ± 0.25 | 91.42 ± 0.48 | 89.09 ± 0.21 |
| 500 | 91.25 ± 1.07 | 87.56 ± 0.35 | 84.77 ± 0.26 | 82.24 ± 0.35 |
| 250 | 87.96 ± 0.62 | 83.88 ± 0.68 | 80.64 ± 0.20 | 75.48 ± 0.36 |
| 125 | 81.09 ± 0.32 | 76.54 ± 0.28 | 71.89 ± 0.36 | 67.14 ± 0.24 |
| 62.5 | 71.41 ± 0.94 | 67.59 ± 0.28 | 65.16 ± 0.31 | 55.53 ± 0.31 |
| 31.25 | 60.79 ± 0.48 | 51.86 ± 0.59 | 49.84 ± 0.15 | 44.98 ± 0.18 |
| 15.62 | 46.51 ± 0.85 | 36.42 ± 0.23 | 34.82 ± 0.33 | 32.61 ± 0.39 |
| 7.81 | 31.77 ± 0.65 | 29.08 ± 0.51 | 27.94 ± 0.27 | 26.09 ± 0.32 |
Fig. 10.

Dose–response curves: percentage bacterial growth inhibition of S. mutans (left panel) and L. acidophilus (right panel) by the Ag-HAp-MSN nanocomposite and individual components (AgNPs, MSNs, n-HAp) across 1000–7.81 µg/mL. The composite consistently produced the highest inhibition at every concentration tested (n = 3; mean ± SD)
Anti-biofilm activity (crystal violet)
The crystal violet biofilm inhibition data are presented in Table 7. The nanocomposite achieved the highest reductions: 82.53 ± 0.16% (S. mutans) and 87.53 ± 0.59% (L. acidophilus) at MBC (Fig. 11). All pairwise comparisons between the composite and individual components were statistically significant (p < 0.001). Even n-HAp, the least potent component, achieved reductions of 72.67% and 76.38%, confirming the independent contributions from all three components. As the assay used a prevention model (test material and inoculum introduced simultaneously), results reflect inhibition of de novo biofilm formation.
Table 7.
Percentage biofilm biomass inhibition at MBC — crystal violet assay (mean ± SD, n = 3)
| Sample | S. mutans (%) | L. acidophilus (%) | Significance (vs. untreated ctrl) |
|---|---|---|---|
| Ag-HAp-MSN | 82.53 ± 0.16 | 87.53 ± 0.59 | p < 0.001 |
| AgNPs | 80.10 ± 0.30 | 84.41 ± 1.04 | p < 0.001 |
| MSNs | 76.60 ± 0.86 | 81.37 ± 0.96 | p < 0.001 |
| n-HAp | 72.67 ± 1.18 | 76.38 ± 0.29 | p < 0.001 |
Prevention model: test material and inoculum co-introduced. Percentage reduction relative to untreated control. Crystal violet solubilised in 33% glacial acetic acid; absorbance at 595 nm
Fig. 11.

Percentage biofilm biomass inhibition (crystal violet assay, prevention model) of S. mutans and L. acidophilus by the Ag-HAp-MSN nanocomposite and individual components at MBC. The nanocomposite achieved the highest inhibition against both organisms (82.53% and 87.53%, respectively). All pairwise comparisons vs. individual components: p < 0.001 (n = 3; mean ± SD)
CLSM 3D Z-stack imaging
CLSM 3D Z-stack reconstructions provided qualitative three-dimensional visualisation of biofilm viability. Green fluorescence indicates live cells, while red fluorescence indicates dead or membrane-compromised cells. In untreated controls, dense green fluorescence (live cells) dominated the full biofilm depth for both organisms. Figure 11 shows 3D and 2D CLSM images of GC Tooth Mousse-treated biofilms for both organisms. Figure 12 shows 3D and 2D CLSM images of Ag-HAp-MSN-treated biofilms for both organisms. After GC Tooth Mousse and Ag-HAp-MSN nanocomposite treatment, 3D reconstructions showed near-complete dominance of red fluorescence (dead/membrane-compromised cells) with negligible residual green signal throughout the biofilm z-axis, indicating depth-penetrant bactericidal activity, which was confirmed by 2D cross-sections (Figs. 12 and 13).
Fig. 12.

CLSM Z-stack images of S. mutans (upper panels) and L. acidophilus (lower panels) biofilms after MBC treatment with GC Tooth Mousse. (A, D) Untreated biofilm imaged at depth 20 μm; (B, E) 3D reconstruction images; (C, F) 2D reconstruction images
Fig. 13.

CLSM Z-stack images of S. mutans (upper panels) and L. acidophilus (lower panels) biofilms after MBC treatment with the Ag-HAp-MSN nanocomposite. A, D Untreated biofilm imaged at depth 20 μm; (B, E) 3D reconstruction images; (C, F) 2D reconstruction images
AO/EB fluorescence live/dead quantification
AO/EB quantitative data are in Fig. 14; Table 8. The nanocomposite produced the highest dead-cell fractions: 83.63 ± 0.42% (S. mutans) and 89.33 ± 0.12% (L. acidophilus), both significantly above all individual components and the untreated control (p < 0.001). The untreated control showed > 88% viable cells (AO-positive), confirming assay validity. AO/EB values tracked the crystal violet biofilm inhibition data closely in rank order and magnitude, providing cross-platform corroboration.
Fig. 14.

Quantitative AO/EB live/dead fluorescence analysis of S. mutans and L. acidophilus biofilms after treatment with Ag-HAp-MSN nanocomposite and individual components at MBC. The nanocomposite demonstrated the highest dead-cell fractions against both organisms, consistent with crystal violet and CLSM findings (n = 3)
Table 8.
AO/EB live/dead fluorescence quantification at MBC (Mean ± SD, n = 3)
| Sample | SM Dead (%) | SM Live (%) | LA Dead (%) | LA Live (%) | Significance |
|---|---|---|---|---|---|
| Ag-HAp-MSN | 83.63 ± 0.42 | 16.37 ± 0.42 | 89.33 ± 0.12 | 10.67 ± 0.12 | p < 0.001 |
| AgNPs | 79.73 ± 0.71 | 20.27 ± 0.71 | 85.47 ± 0.65 | 14.53 ± 0.65 | p < 0.001 |
| MSNs | 75.03 ± 0.86 | 24.97 ± 0.86 | 80.73 ± 0.90 | 19.27 ± 0.90 | p < 0.001 |
| n-HAp | 73.27 ± 0.57 | 26.73 ± 0.57 | 78.10 ± 0.46 | 21.90 ± 0.46 | p < 0.001 |
| Control (untreated) | 10.07 ± 0.25 | 89.93 ± 0.25 | 11.30 ± 0.62 | 88.70 ± 0.62 | — |
Dead = EB-positive (red); Live = AO-positive (green). p-values vs. untreated control; one-way ANOVA with Tukey post-hoc. Simbioen Labs, inverted epifluorescence microscope, ImageJ quantification
Discussion
The nanocomposite demonstrated significantly higher activity than its individual components across all experimental endpoints (p < 0.001). At higher concentrations, the nanocomposite demonstrated antibacterial efficacy against L. acidophilus comparable to GC Tooth Mousse, but reduced efficacy was observed with S. mutans, which is consistent with the resilience of this organism. The antibacterial effect likely results from multiple simultaneous mechanisms (Fig. 15).
Fig. 15.

Proposed multimodal antibacterial and anti-biofilm mechanism of the Ag-HAp-MSN nanocomposite illustrating: (i) Ag⁺ ion release causing membrane disruption; (ii) ROS-mediated intracellular oxidative stress; (iii) DNA/enzyme inhibition; (iv) Ca²⁺/PO₄³⁻ ion release from n-HAp supporting enamel remineralisation; and (v) MSN mesopore scaffold-mediated Ag⁺ release, hypothesized to be sustained based on intact mesopore architecture, enabling deep EPS matrix penetration. The five components correspond to the five mechanistic pathways discussed in Sect. 4
Silver ions have the ability to destabilize bacterial membranes, disrupt intracellular processes, and induce oxidative stress [8–10]. BET analysis confirmed the preservation of mesoporosity, which is hypothesized to facilitate ion diffusion through the biofilm matrix, although this was not directly measured in the present study. CLSM investigations showed that bactericidal activity was demonstrated throughout the entire depth of the biofilm, and not only on the upper layers. The system may also be enhanced by the addition of n-HAp, which is expected to release Ca²⁺ and PO₄³⁻ ions and could influence bacterial adhesion and the remineralisation process, although direct ion-release measurements were not performed in this study. The band observed in the FTIR at approximately 490 cm⁻¹ provides additional information on structural organization. The fact that only silver atoms are present in the composite suggests the coordination of the atom with oxygen-bearing groups in the matrix, in agreement with the previously reported vibrational modes in similar systems [34].
The zeta potential of the composite was measured at − 9.22 mV. This value is well below the conventional ± 30 mV threshold used to define the electrostatic colloidal stability. This represents a potential limitation. Saliva is an ion-rich environment containing calcium, phosphate, and proteins that may destabilize weakly charged particles and promote aggregation. During the 24–48-hour incubations used in this study, some degree of aggregation may have occurred, potentially leading to slight underestimation of the activity of fully dispersed particles. The phytochemical corona derived from Cissus quadrangularis may also contribute partial steric stabilization. Further research is necessary to measure the stability of the particles under the assay conditions using time-resolved DLS measurements in BHI broth. Therefore, any route to in-vivo assessment should emphasize the surface stabilisation. Several strategies should be considered. PEGylation is the most established method for silica-based nanocarriers, offering steric protection without interfering with the core structure. Chitosan coating would be a particularly appealing choice in this environment as they would accomplish two tasks at once: changing the zeta potential to the positive stable range and introducing its own antibacterial nature, which is specifically applicable to an oral usage [35].
In comparison to the previous studies on silver nanoparticles, Hernandez-Sierra et al. reported that MIC values of 100–500 µg/mL of simple AgNPs against S. mutans [36], and Perez-Diaz et al. reported ZOI values of 14–18 mm of AgNPs at the same doses [37]. At a concentration of 1000 µg/mL, our composite had ZOI values of 25 mm with S. mutans and 29 mm with L. acidophilus, a 2-4-fold reduction of MIC in the composite compared to the individual components. Similar findings have been reported for other multicomponent silver systems [38, 39]. Formal synergy testing (FICI analysis) was not performed in this study; without these, the nature of interactions that occur between the components (synergistic, additive, or indifferent) cannot be determined.
AgNPs generally produced larger ZOI values than MSN and n-HAp, whereas the MIC and MBC values were comparable between AgNPs and MSN for both organisms, with higher MBC requirements observed for n-HAp against L. acidophilus (Table 4). This should not be interpreted as MSN and n-HAp possessing antibacterial potency equivalent to AgNPs; rather, the three materials exhibited measurable activity under the specific conditions of this assay. AgNPs are well established to exert antibacterial effects through Ag⁺-mediated toxicity, oxidative stress, membrane disruption, and DNA damage [8–10]. The present AgNPs showed a Scherrer crystallite size of 165 nm and a zeta potential of − 34.7 mV, with FTIR evidence of surface-associated Cissus quadrangularis-derived functional groups; although Ag⁺ release kinetics were not directly measured, these physicochemical characteristics may influence particle–bacteria interactions and silver bioavailability [40]. MSNs are generally regarded as nanocarrier materials, but their biological behaviour can be influenced by particle size, morphology, surface chemistry and surface charge, and residual CTAB has been shown to contribute substantially to the antibacterial toxicity of MSN preparations when the surfactant is incompletely removed [41]; residual CTAB was not independently quantified in the present study, so its contribution to the observed MSN activity remains a possible but unconfirmed factor. Calcium phosphate and hydroxyapatite nanoparticles can similarly exhibit measurable antimicrobial effects through mechanisms involving particle size, solubility, surface properties and interactions with bacterial membranes [42, 43], so the activity observed for n-HAp is biologically plausible, although material- and condition-dependent and mechanistically distinct from silver-mediated action. Furthermore, ZOI is a diffusion-based endpoint influenced by particle dispersion, aggregation and diffusivity through the agar matrix, so comparable ZOI values among materials should not be read as evidence of equivalent intrinsic antibacterial potency. Component-resolved BET surface-area and dissolution/solubility measurements for the individual MSN and n-HAp components were not obtained in the present study, as BET analysis was performed only on the final nanocomposite; this is identified as a limitation to be addressed with time-resolved ion-release and surface-area studies in future work.
These biofilm findings are clinically relevant because biofilm-associated bacteria are more resistant than planktonic cells [44]. The crystal violet assay has been developed as a preventative paradigm, therefore, the inhibitions of 82.53% and 87.53 represents the inhibition of de novo biofilm formation, and not the elimination of an existing biofilm. These data were monitored using AO/EB fluorescence (83.63% and 89.33% dead cell percentages) providing cross-platform validation using two different instruments and two different dye systems [35, 45]. CLSM 3D imaging visually confirmed depth-penetrant bactericidal activity throughout the biofilm architecture.
The MBC values used in the biofilm-prevention assay were determined against planktonic cells and should therefore not be regarded as equivalent to the concentration required to eradicate an established biofilm; this distinction between the minimum bactericidal concentration for planktonic cells (MBC-P) and for biofilm cells (MBC-B) is described in the literature [46], and biofilm-associated bacteria can show markedly reduced antimicrobial susceptibility due to extracellular matrix interactions, altered metabolic state, and other biofilm-specific tolerance mechanisms [47]. Because the crystal violet assay was a prevention model in which the test material and bacterial inoculum were introduced simultaneously, residual biofilm biomass at the respective planktonic MBC does not contradict the MIC/MBC results; the inhibition percentages, which remained below 100% for all materials, reflect inhibition of de novo biofilm biomass formation rather than eradication of an established biofilm. Each material was tested at its own respective MBC rather than at a common concentration, so the resulting biofilm inhibition percentages reflect the performance of each material under its own MBC condition and should not be interpreted as concentration-matched comparisons of intrinsic antibiofilm potency; a concentration-matched dose–response study together with determination of biofilm-specific bactericidal concentrations (MBC-B) would be required for such a comparison.
GC Tooth Mousse is a widely used CPP-ACP agent in clinical practice and is not primarily designed as an antibacterial material [48]. The observed statistically comparable ZOI against L. acidophilus under agar diffusion conditions should be interpreted as an exploratory contextual comparison rather than direct therapeutic equivalence. Collectively, the demonstrated antibacterial activity (MIC/MBC), anti-biofilm inhibition, and remineralization potential of the nanocomposite support its further evaluation as an adjunctive anticariogenic material rather than a direct substitute for CPP-ACP products [49–55].
Several limitations of this study should be acknowledged. A key limitation is the absence of direct Ag⁺ release kinetics data, which is required to comprehensively validate the hypothesized sustained-release mechanism, future dosage optimization, and safety evaluation related to oral mucosal and systemic exposure. The sustained-release argument currently rests on indirect evidence—the BET-confirmed intact mesopore network and published behaviour of analogous Ag@SiO₂ systems [34, 49]; however, this does not replace direct release quantification. Quantitative Ag⁺ profiling by ICP-OES at time points of 1, 4, 8, 24, 48, and 72 h in simulated oral fluid at 37 °C should be prioritized in future studies. Furthermore, the study used monospecies bacterial models that cannot fully replicate the polymicrobial ecology of natural dental plaque [44, 52]. The GC Tooth Mousse comparison was conducted at a separate institution (Green Lab, Saveetha Dental College and Hospital, SIMATS) from the main antibacterial panel (Simbioen). Although the concentration equivalence was established through well-volume normalization, this remains an indirect comparison. The MIC and MBC of GC Tooth Mousse could not be determined because its viscous cream formulation is incompatible with broth microdilution. The ZOI, MIC, and MBC are independent endpoints measured under different assay geometries (diffusion-based vs. dilution-based), so a given concentration’s ZOI value is not expected to scale linearly or predictably with its MIC/MBC classification. The apparent “larger ZOI at MIC” reflects the fact that ZOI reflects a bacteriostatic threshold visible at the diffusion front, while MIC/MBC are measured in a fully mixed liquid system; these are complementary but methodologically distinct measures, and no fixed proportional relationship between them is claimed.
Finally, the marginal zeta potential must be characterised over time with DLS in a simulated oral fluid before any storage stability claim can be made. The next priority steps include comprehensive Ag⁺ release kinetics profiling by ICP-OES and advanced surface stabilisation strategies to achieve colloidal stability in complex biological environments which address the most fundamental nanoscience gaps identified. Further investigation into polymicrobial and eradication-model biofilm studies, cytotoxicity at effective concentrations, and in vivo biocompatibility will be essential before eventual translation into appropriate dental delivery formats. Our previous study also demonstrated cytocompatibility in pulp stem cells, supporting further translational investigation [32]. The convergence of physicochemical characterisation and multi-assay biological validation across two independent laboratories underscores the robustness of the observed antibacterial and anti-biofilm effects.
Conclusion
The Cissus quadrangularis-mediated biogenic Ag-HAp-MSN nanocomposite was evaluated for anti-cariogenic activity against Streptococcus mutans and Lactobacillus acidophilus using a five-assay panel: ZOI, MIC, MBC, crystal violet biofilm biomass inhibition, and AO/EB fluorescence live/dead quantification, supplemented with CLSM 3D Z-stack imaging. Batch-reconfirmed physicochemical characterisation confirmed successful tripartite assembly with intact mesopore architecture (BET 108.0 m²/g; pore diameter 10.68 nm; zeta potential − 9.22 mV) and possible inter-component interactions (novel FTIR band ~ 490 cm⁻¹). Across the quantitative assays (ZOI, MIC, MBC, and biofilm biomass inhibition), the composite significantly outperformed the three individual components (p < 0.001), with complementary qualitative CLSM and AO/EB imaging further supporting depth-penetrant bactericidal activity. Biofilm biomass inhibition reached 87.53% and AO/EB dead cell quantification showed 89.33% bactericidal cell death for L. acidophilus; CLSM 3D imaging confirmed depth-penetrant bactericidal activity throughout the full biofilm z-axis.
The nanocomposite demonstrated strong antibacterial and anti-biofilm activity while retaining the remineralization potential of the n-HAp component. Although the comparison of GC Tooth Mousse should be interpreted cautiously due to the formulation differences, the findings support further preclinical evaluation of this material. Future research should focus on Ag⁺ release profiling, colloidal stability, polymicrobial biofilm models, and formulation development.
Supplementary information
Below is the link to the electronic supplementary material.
Acknowledgements
The authors acknowledge the SRM Central Instrumentation Facility (SCIF) and Nanotechnology Research Centre (NRC), SRMIST, Kattankulathur, Chengalpattu, Tamil Nadu, India, for the instrumentation access. The authors gratefully acknowledge Simbioen Labs and Scientific Services Private Limited, Chennai (SBTW/13/12/020), for technical support with the ZOI, MIC, MBC, and AO/EB fluorescence antibacterial panel; and Saveetha Dental College and Hospital, SIMATS, Chennai, Tamil Nadu, India, for CLSM 3D Z-stack imaging and the GC Tooth Mousse comparative ZOI study. The authors gratefully acknowledge the financial support by SRM Kattankulathur Dental College and Hospital, Faculty of Medicine and Health Sciences, SRM Institute of Science and Technology, Kattankulathur, Chengalpattu, Tamil Nadu, India, for bearing the defrayed costs of publishing this article.
Author contributions
S.K.: Conceptualization, antimicrobial and biofilm assays, data interpretation, and manuscript drafting and editing. V.V.N.: Conceptualization, supervision, manuscript review and editing, and validation. M.S.: Data analysis, data interpretation, manuscript drafting, and editing. S.A.: Nanoparticle synthesis, characterization, data analysis, and interpretation. V.V.K.: Manuscript review and editing, supervision. All authors read and approved the final manuscript.
Funding
Open access funding provided by SRM Institute of Science and Technology for SRMIST – Medical & Health Sciences. This research received no external funding from any public, commercial, or not-for-profit funding agency.
Data availability
All data supporting the conclusions of this article are fully presented within the manuscript. Raw laboratory report data (Simbioen Labs, SBTW/13/12/020) are available from the corresponding author on reasonable request.
Declarations
Ethics approval and plant collection statement
Fresh stems of Cissus quadrangularis were commercially procured from certified organic farms in and around Chennai (12.97°N, 80.22°E) and Kancheepuram (12.83°N, 79.70°E), Tamil Nadu, India. This plant is widely cultivated in Tamil Nadu and is not a wild or protected species. Since the plant material was not collected from wild populations, herbarium deposition and voucher specimen requirements were not applicable to this study. The plant material was authenticated by the School of Life Sciences, SRM Institute of Science and Technology, Kattankulathur, Chengalpattu, Tamil Nadu, India (Authentication Ref: SRM-BOT-2024-12). All procurement and use complied with applicable local and national guidelines of India. This study did not involve human participants, vertebrate animals, or protected plant species.
Consent for publication
Not applicable.
Consent to participate
Not applicable.
Clinical trial number
Not applicable.
Competing interests
The authors declare no competing interests.
Supplementary Information
The online version contains supplementary material available at https://doi.org/10.1186/s11671-026-05153-w.
Footnotes
Publisher’s note
Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.
Contributor Information
Shobana Krishnakumar, Email: shobanak1@srmist.edu.in.
Vidyashree Nandini Venugopal, Email: vidyashv@srmist.edu.in.
References
- 1.Takahashi H, Nadres ET, Kuroda K. Cationic amphiphilic polymers with antimicrobial activity for oral care applications: eradication of S. mutans biofilm. Biomacromolecules. 2017;18:257–65. 10.1021/acs.biomac.6b01598. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 2.Selwitz RH, Ismail AI, Pitts NB. Dental caries. Lancet. 2007;369:51–9. 10.1016/S0140-6736(07)60031-2. [DOI] [PubMed] [Google Scholar]
- 3.Alasraj AF, Alasimi OM, Alturki AA, Almatrouk WF, Alhazzaa NA, Almutairi BH, et al. Dental caries as a biofilm-mediated disease: current concepts and emerging therapies. Rev Diabet Stud. 2024;20:64–78. 10.70082/s29zqs86. [DOI] [Google Scholar]
- 4.Marsh PD. Dental plaque as a biofilm and a microbial community - implications for health and disease. BMC Oral Health. 2006;6:S14. 10.1186/1472-6831-6-S1-S14. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 5.Takahashi N, Nyvad B. The role of bacteria in the caries process: ecological perspectives. J Dent Res. 2011;90:294–303. 10.1177/0022034510379602. [DOI] [PubMed] [Google Scholar]
- 6.Reynolds EC. Casein phosphopeptide-amorphous calcium phosphate: the scientific evidence. Adv Dent Res. 2009;21:25–9. 10.1177/0895937409335619. [DOI] [PubMed] [Google Scholar]
- 7.Moussa DG, Ahmad P, Mansour TA, Siqueira WL. Current state and challenges of the global outcomes of dental caries research in the meta-omics era. Front Cell Infect Microbiol. 2022;12:887907. 10.3389/fcimb.2022.887907. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 8.Gamea S, Radvar E, Athanasiadou D, Chan RL, De Sero G, Ware E, et al. Biomimetic mineralization of keratin scaffolds for enamel regeneration. Adv Healthc Mater. 2025;14:e02465. 10.1002/adhm.202502465. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 9.Rai M, Yadav A, Gade A. Silver nanoparticles as a new generation of antimicrobials. Biotechnol Adv. 2009;27:76–83. 10.1016/j.biotechadv.2008.09.002. [DOI] [PubMed] [Google Scholar]
- 10.Noronha VT, Paula AJ, Durán G, Galembeck A, Cogo-Müller K, Franz-Montan M, Durán N. Silver nanoparticles in dentistry. Dent Mater. 2017;33:1110–26. 10.1016/j.dental.2017.07.002. [DOI] [PubMed] [Google Scholar]
- 11.Revathi S, Sutikno S, Hasan AF, Altemimi AB, ALKaisy QH, Phillips AJ, et al. Green synthesis and characterization of silver nanoparticles (AgNP) using Acacia nilotica plant extract and their anti-bacterial activity. Food Chem Adv. 2024;4:100680. 10.1016/j.focha.2024.100680. [DOI] [Google Scholar]
- 12.Widatalla HA, Yassin LF, Alrasheid AA, Rahman Ahmed SA, Widdatallah MO, Eltilib SH, et al. Green synthesis of silver nanoparticles using green tea leaf extract, characterization and evaluation of antimicrobial activity. Nanoscale Adv. 2022;4:911–5. 10.1039/d1na00509j. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 13.Zhao R, Meng X, Pan Z, Li Y, Qian H, Zhu X, et al. Advancements in nanohydroxyapatite: synthesis, biomedical applications and composite developments. Regen Biomater. 2024;12:rbae129. 10.1093/rb/rbae129. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 14.Piecuch A, Targońska S, Rewak-Sorczyńska J, Ogórek R, Wiglusz RJ. New silicate-substituted hydroxyapatite materials doped with silver ions as potential antifungal agents. BMC Microbiol. 2023;23:193. 10.1186/s12866-023-02930-w. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 15.Jiang J, Liu W, Xiong Z, Hu Y, Xiao J. Effects of biomimetic hydroxyapatite coatings on osteoimmunomodulation. Biomater Adv. 2022;134:112640. 10.1016/j.msec.2021.112640. [DOI] [PubMed] [Google Scholar]
- 16.Sousa A, Souza KC, Sousa EM. Mesoporous silica/apatite nanocomposite: special synthesis route to control local drug delivery. Acta Biomater. 2008;4:671–9. 10.1016/j.actbio.2007.11.003. [DOI] [PubMed] [Google Scholar]
- 17.Mourhly A, Khachani M, Hamidi AE, Kacimi M, Halim M, Arsalane S. The synthesis and characterization of low-cost mesoporous silica SiO2 from local pumice rock. Nanomaterials Nanatechnol. 2015;5:35. 10.5772/62033. [DOI] [Google Scholar]
- 18.Vivero-Escoto JL, Slowing II, Trewyn BG, Lin VS. Mesoporous silica nanoparticles for intracellular controlled drug delivery. Small. 2010;6:1952–67. 10.1002/smll.200901789. [DOI] [PubMed] [Google Scholar]
- 19.Fotie J. Applications of tailored mesoporous silicate nanomaterials in regenerative medicine and theranostics. Int J Mol Sci. 2025;26:7918. 10.3390/ijms26167918. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 20.Maghimaa M, Alharbi SA. Green synthesis of silver nanoparticles from Curcuma longa L. and coating on the cotton fabrics for antimicrobial applications and wound healing activity. J Photochem Photobiol B. 2020;204:111806. 10.1016/j.jphotobiol.2020.111806. [DOI] [PubMed] [Google Scholar]
- 21.Duraisamy R, Arizo A, Yilma B. Antibacterial and antioxidant activity of plant-mediated green synthesized silver nanoparticles using Cissus quadrangularis aqueous extract. Bull Chem Soc Ethiop. 2025;39:483–502. 10.4314/bcse.v39i3.8. [DOI] [Google Scholar]
- 22.Valli JS, Vaseeharan B. Biosynthesis of silver nanoparticles by Cissus quadrangularis extracts. Mater Lett. 2012;82:171–3. 10.1016/j.matlet.2012.05.040. [DOI] [Google Scholar]
- 23.Rajeshkumar S, Menon S, SVK, Ponnanikajamideen M, Ali D, Arunachalam K. Anti-inflammatory and antimicrobial potential of Cissus quadrangularis‐assisted copper oxide nanoparticles. J Nanomaterials. 2021;2021:5742981. 10.1155/2021/5742981. [DOI] [Google Scholar]
- 24.Santhoshkumar T, Rahuman AA, Bagavan A, Marimuthu S, Jayaseelan C, Kirthi AV, et al. Evaluation of stem aqueous extract and synthesized silver nanoparticles using Cissus quadrangularis against Hippobosca maculata and Rhipicephalus (Boophilus) microplus. Exp Parasitol. 2012;132:156–65. 10.1016/j.exppara.2012.06.009. [DOI] [PubMed] [Google Scholar]
- 25.Tabari K, Hosseinpour S, Parashos P, Kardouni Khozestani P, Rahimi HM. Cytotoxicity of selected nanoparticles on human dental pulp stem cells. Iran Endod J. 2017;12:137–42. 10.22037/iej.2017.28. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 26.Rodrigues MC, Rolim WR, Viana MM, Souza TR, Gonçalves F, Tanaka CJ, et al. Biogenic synthesis and antimicrobial activity of silica-coated silver nanoparticles for esthetic dental applications. J Dent. 2020;96:103327. 10.1016/j.jdent.2020.103327. [DOI] [PubMed] [Google Scholar]
- 27.Ni Z, Gu X, He Y, Wang Z, Zou X, Zhao Y, et al. Synthesis of silver nanoparticle-decorated hydroxyapatite (HA@Ag) poriferous nanocomposites and the study of their antibacterial activities. RSC Adv. 2018;8:41722–30. 10.1039/c8ra08148d. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 28.Mallineni SK, Sakhamuri S, Kotha SL, AlAsmari ARGM, AlJefri GH, Almotawah FN, et al. Silver nanoparticles in dental applications: a descriptive review. Bioeng (Basel). 2023;10:327. 10.3390/bioengineering10030327. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 29.Alkhazaleh A, Elfagih S, Chakka LRJ, Armstrong SR, Comnick CL, Qian F, et al. Development of proanthocyanidin-loaded mesoporous silica nanoparticles for improving dental adhesion. Mol Pharm. 2022;19:4675–84. 10.1021/acs.molpharmaceut.2c00728. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 30.Aguilar-García D, Ochoa-Terán A, Paraguay-Delgado F, Díaz-García ME, Pina-Luis G. Water-compatible core–shell Ag@SiO2 molecularly imprinted particles for the controlled release of tetracycline. J Mater Sci. 2016;51:5651–63. 10.1007/s10853-016-9867-x. [DOI] [Google Scholar]
- 31.Izzetti R, Gennai S, Nisi M, Gulia F, Miceli M, Giuca MR. Clinical applications of nano-hydroxyapatite in dentistry. Appl Sci. 2022;12:10762. 10.3390/app122110762. [DOI] [Google Scholar]
- 32.Krishnakumar S, Nandini VV, Thirunavukarasu K, Chinnathambi U, Venkatesh KV. Cissus quadrangularis mediated biogenic synthesis of silver-nanohydroxyapatite-mesoporous silica nanocomposite, characterization, and cytotoxicity evaluation on dental pulp stem cells. Discov Nano. 2025;20:150. 10.1186/s11671-025-04336-1. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 33.Patterson AL. The Scherrer formula for X-Ray particle size determination. Phys Rev. 1939;56:978–82. 10.1103/PhysRev.56.978. [DOI] [Google Scholar]
- 34.Devi P, Patil SD, Jeevanandam P, Navani NK, Singla ML. Synthesis, characterization and bactericidal activity of silica/silver core-shell nanoparticles. J Mater Sci Mater Med. 2014;25:1267–73. 10.1007/s10856-014-5165-9. [DOI] [PubMed] [Google Scholar]
- 35.Leng D, Li Y, Zhu J, Liang R, Zhang C, Zhou Y, Li M, Wang Y, Rong D, Wu D, Li J. The antibiofilm activity and mechanism of nanosilver- and nanozinc-incorporated mesoporous calcium-silicate nanoparticles. Int J Nanomed. 2020;15:3921–36. 10.2147/IJN.S244686. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 36.Hernández-Sierra JF, Ruiz F, Pena DC, Martínez-Gutiérrez F, Martínez AE, Guillén Ade J, et al. The antimicrobial sensitivity of Streptococcus mutans to nanoparticles of silver, zinc oxide, and gold. Nanomedicine. 2008;4:237–40. 10.1016/j.nano.2008.04.005. [DOI] [PubMed] [Google Scholar]
- 37.Pérez-Díaz MA, Boegli L, James G, Velasquillo C, Sánchez-Sánchez R, Martínez-Martínez RE, et al. Silver nanoparticles with antimicrobial activities against Streptococcus mutans and their cytotoxic effect. Mater Sci Eng C Mater Biol Appl. 2015;55:360–6. 10.1016/j.msec.2015.05.036. [DOI] [PubMed] [Google Scholar]
- 38.Sharma P, Dhawan P, Rajpal SK, Sharma R. A comparison of antimicrobial efficacy of silver-based preventive restorations (silver nitrate, silver diamine fluoride, and silver nanoparticles) against Streptococcus mutans monospecies biofilm model. Int J Clin Pediatr Dent. 2023;16:S13–9. 10.5005/jp-journals-10005-2575. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 39.Laredo-Naranjo MA, Carrillo-Gonzalez R, De La Garza-Ramos MA, Garza-Navarro MA, Torre-Martinez HHH, Del Angel-Mosqueda C, et al. Antimicrobial properties and dental pulp stem cell cytotoxicity using carboxymethyl cellulose-silver nanoparticles deposited on titanium plates. Acta Biomater Odontol Scand. 2016;2:60–7. 10.3109/23337931.2016.1160783. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 40.More PR, Pandit S, De Filippis A, Franci G, Mijakovic I, Galdiero M. Silver Nanoparticles: Bactericidal and mechanistic approach against drug resistant pathogens. Microorganisms. 2023;11:369. 10.3390/microorganisms11020369. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 41.Son MJ, Lee SW. Antibacterial toxicity of mesoporous silica nanoparticles with functional decoration of specific organic moieties. Colloids Surf Physicochem Eng Asp. 2021;630:127612. 10.1016/j.colsurfa.2021.127612. [DOI] [Google Scholar]
- 42.Wu VM, Huynh E, Tang S, Uskoković V. Calcium phosphate nanoparticles as intrinsic inorganic antimicrobials: mechanism of action. Biomed Mater. 2021;16:015018. 10.1088/1748-605X/aba281. [DOI] [PubMed] [Google Scholar]
- 43.Uskoković V, Tang S, Nikolić MG, Marković S, Wu VM. Calcium phosphate nanoparticles as intrinsic inorganic antimicrobials: In search of the key particle property. Biointerphases. 2019;14:031001. 10.1116/1.5090396. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 44.Zhang K, Li X, Yu C, Wang Y. Promising therapeutic strategies against microbial biofilm challenges. Front Cell Infect Microbiol. 2020;10:359. 10.3389/fcimb.2020.00359. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 45.McBain AJ. Chapter 4: In vitro biofilm models: an overview. Adv Appl Microbiol. 2009;69:99–132. 10.1016/S0065-2164(09)69004-3. [DOI] [PubMed] [Google Scholar]
- 46.Mah TF. Establishing the minimal bactericidal concentration of an antimicrobial agent for planktonic cells (MBC-P) and biofilm cells (MBC-B). J Vis Exp. 2014;83e50854. 10.3791/50854. [DOI] [PMC free article] [PubMed]
- 47.Hall CW, Mah TF. Molecular mechanisms of biofilm-based antibiotic resistance and tolerance in pathogenic bacteria. FEMS Microbiol Rev. 2017;41:276–301. 10.1093/femsre/fux010. [DOI] [PubMed] [Google Scholar]
- 48.Abufarwa M, Noureldin A, Dziak R, Covell D. Efficacy of CPP-ACP fluoride varnish applied with and without acid etching in preventing enamel demineralization compared to light-curable fluoride varnish. Angle Orthod. 2022;92:213–9. 10.2319/050121-345.1. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 49.Agnihotri S, Mukherji S, Mukherji S. Immobilized silver nanoparticles enhance contact killing and show highest efficacy: elucidation of the mechanism of bactericidal action of silver. Nanoscale. 2013;5:7328–40. 10.1039/c3nr00024a. [DOI] [PubMed] [Google Scholar]
- 50.Guzman M, Dille J, Godet S. Synthesis and antibacterial activity of silver nanoparticles against gram-positive and gram-negative bacteria. Nanomedicine. 2012;8:37–45. 10.1016/j.nano.2011.05.007. [DOI] [PubMed] [Google Scholar]
- 51.Roe D, Karandikar B, Bonn-Savage N, Gibbins B, Roullet JB. Antimicrobial surface functionalization of plastic catheters by silver nanoparticles. J Antimicrob Chemother. 2008;61:869–76. 10.1093/jac/dkn034. [DOI] [PubMed] [Google Scholar]
- 52.Al-Ansari MM, Al-Dahmash ND, Ranjitsingh AJA. Synthesis of silver nanoparticles using gum Arabic: Evaluation of its inhibitory action on Streptococcus mutans causing dental caries and endocarditis. J Infect Public Health. 2021;14(3):324–30. 10.1016/j.jiph.2020.12.016. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 53.Barakat NAM, Khalil KA, Sheikh FA, Omran AM, Gaihre B, Khil MS. Physiochemical characterizations of hydroxyapatite extracted from bovine bones by three different methods: extraction of biologically desirable. Hap Mater Sci Eng C. 2008;28:1381–7. https://hdl.handle.net/10779/uow.27750717.v1. [Google Scholar]
- 54.Mondal S, Mondal B, Dey A, Mukhopadhyay SS. Studies on processing and characterization of hydroxyapatite biomaterials from different bio wastes. J Min Mater Charact Eng. 2012;11:55–67. 10.4236/jmmce.2012.111005. [DOI] [Google Scholar]
- 55.Hooi MT, Phang SW, Yow HY, David E, Kim NX, Choo HL. FTIR spectroscopy characterization and critical comparison of poly (vinyl) alcohol and natural hydroxyapatite derived from fish bone composite for bone-scaffold. In Journal of Physics: Conference Series. 2021; 2120: 012004. 10.1088/1742-6596/2120/1/012004 [DOI]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Supplementary Materials
Data Availability Statement
All data supporting the conclusions of this article are fully presented within the manuscript. Raw laboratory report data (Simbioen Labs, SBTW/13/12/020) are available from the corresponding author on reasonable request.