Skip to main content
RSC Advances logoLink to RSC Advances
. 2026 Nov 24. Online ahead of print. doi: 10.1039/d6ra07029a

SnFe2O4–rGO heterojunction for visible light driven photocatalytic degradation of methylene blue: a combined experimental and theoretical study

Vani Narayanan a, Giridhar Baburao a, Amey Anant Joshi a, Badal Kumar Mandal a, Gopi Ragupathy a,✉
PMCID: PMC13795331  PMID: 43081146

Abstract

The widespread use of methylene blue (MB) in industrial processes and its subsequent release into aquatic environments necessitate effective removal strategies. In this study, a novel composite material was synthesized via co-precipitation by integrating tin–iron oxide (SnFe2O4) with reduced graphene oxide (rGO) to enhance the photodegradation of MB under visible light. The incorporation of rGO plays a crucial role in improving the photocatalytic performance by providing a conductive pathway for efficient electron transport, facilitating charge separation, and suppressing electron–hole recombination. The composite achieved a maximum removal efficiency of 60–70% for MB under optimal conditions. This enhancement is attributed to improved charge transport and reduced energy loss at the interface of the composite components. Computational analyses indicated that the SnFe2O4–rGO composite exhibits superior visible light absorption and electrical conductivity compared to pristine SnFe2O4. These findings demonstrate that the SnFe2O4–rGO composite is a safe and effective material for the removal of methylene blue and related contaminants from water.


The widespread industrial application of methylene blue (MB) and its persistent presence in aquatic environments necessitate the development of innovative approaches, such as visible-light-driven photocatalytic degradation, for effective removal.graphic file with name d6ra07029a-ga.webp

1. Introduction

The discharge of wastewater into the environment is a significant contributor to increasing pollution levels. Specifically, wastewater from the textile industry is a major source of water pollution, adversely impacting aquatic ecosystems. These effluents contain both organic and inorganic pigments, many of which are classified as toxic.1 Furthermore, textile industries consume large quantities of water and release equivalent volumes of contaminated wastewater. Among the pollutants present, Methylene Blue (MB), a common cationic dye, is frequently detected in these effluents. Over time, MB produces toxic byproducts, such as amines and phenols, which have been reported to be highly toxic and are associated with carcinogenicity and gene mutations.2,3 The complex molecular structure and high stability of these dyes further contribute to their resistance to various physical, chemical, and biological remediation techniques.4,5 Additionally, coloured organic dyes in textile effluents hinder sunlight penetration and lower dissolved oxygen levels, rendering the water unsuitable for environmental use. As a result, numerous efforts have been undertaken to treat textile industry wastewater containing toxic and carcinogenic organic dyes.6,7 However, currently available physical, chemical, and biological treatment methods for textile wastewater are often time-consuming, involve complex processes, or require economically prohibitive setups.8 A significant limitation of most existing treatment techniques is the generation of toxic sediments or sludge as secondary pollutants, necessitating additional treatment. In response to these challenges, recent advancements in wastewater treatment have introduced various methods, including green technologies that utilize microbe-based processes.9,10

Photocatalysis has emerged as the predominant method for degrading dyes in wastewater, surpassing other treatment techniques such as absorption, adsorption, thermal catalysis, and anodic breakdown.11,12 This preference is attributed to its lower energy consumption, catalytic stability, and environmental sustainability. The process relies on oxidation as its core mechanism and requires a high-intensity light source and an oxidant to generate hydroxyl radicals.13,14 When exposed to a high-energy light source, the photocatalyst generates electron–hole pairs. These pairs facilitate the production of hydroxyl radicals, which subsequently degrade dye compounds.15 Some of the most widely studied photocatalysts for contaminant removal include wide band gap metal oxide semiconductors such as TiO2, Fe2O3, CoO, Ga2O3, In2O3, WO3, ZrO2 and NiO.16,17 Furthermore, several investigations involving metal oxides and supported systems have demonstrated that newly generated interfacial phases, including spinel and perovskite structures, play a key role in determining the catalytic efficiency.18 Spinels are frequently favoured over binary oxides because they exhibit higher structural and greater thermal stability under severe conditions commonly employed in industrial processes.19

Spinels with the general formula AB2O4 exhibit multiple transition-metal-oxide behaviours and are widely used in catalytic applications. These materials are considered environmentally friendly and less hazardous than noble metal oxides because they have high conductivity and a larger surface area.20,21 Spinel ferrites with various metal combinations, such as CoFe2O4, SnFe2O4, and MnFe2O4, have been demonstrated as a promising material for catalysis, electrochemical sensors and supercapacitors research.22,23 These materials are considered promising nanomaterials for catalysis research due to their diverse physicochemical properties arising from the presence of M2+ and Fe3+ cations.24,25

SnFe2O4 (SFO), an inverted spinel, has attracted significant attention because it exhibits low toxicity and facilitates facile synthesis.26 They exist with Sn2+ cations in octahedral sites and Fe3+ ions in both tetrahedral and octahedral sites.27 SnFe2O4 shows strong visible-light absorption and luminescence, making it a candidate for solar energy harvesting and electro-optical devices.28 It is a stable, tuneable p-type semiconductor with a bandgap active in longer wavelengths.29 Its conduction band is more negative than the O2/˙O2− redox potential, thereby promoting highly reactive superoxide radicals (˙O2−), which are crucial for photocatalytic reactions under visible light. The presence of Fe3+ enables their easy separation after each catalytic use, supporting commercial applicability. However, poor dispersion and potential toxicity remain major challenges.30–32

To overcome these drawbacks and enhance their photocatalytic efficiency, hybridization with reduced graphene oxide (rGO) has emerged as an effective approach. rGO, a two-dimensional carbon material with a layered structure and residual oxygen-containing functional groups, offers a large surface area, enhanced optical properties, and high charge-transfer properties in the resulting nanocomposite.33 The combination of SnFe2O4 with rGO results in a hybrid material, SnFe2O4–rGO (SFO–rGO), whose physicochemical properties are significantly influenced by the synthesis conditions. It is reported that SnFe2O4–rGO is a very promising photocatalyst that demonstrates excellent performance when exposed to ultraviolet (UV) or visible light during the process of photocatalysis. Nevertheless, the catalytic activity of the material is impeded when it is only exposed to visible light because of its high bandgap energy and quick recombination of holes and electrons. This implies substantial restrictions on its practical use. This improves physical as well as visible features of materials.34

Therefore, this study was designed to synthesize and characterize the SnFe2O4–rGO nanocomposite and evaluate its photocatalytic performance for the degradation of MB under simulated visible light. The introduction of rGO to SnFe2O4 is expected to improve the structural, optical, and magnetic properties of the nanocomposite, thereby enhancing its photocatalytic activity. In summary, SnFe2O4–rGO, possessing a lower band gap energy and high surface area, is a suitable candidate for various environmental remediation processes.

2. Experimental work

2.1. Materials

All chemicals and reagents used in the experiments were of analytical grade and employed without further purification. Potassium permanganate (KMnO4), hydrogen peroxide (H2O2), tin(ii) chloride dihydrate (SnCl2·2H2O), and methylene blue (C16H18ClN3S) were sourced from SD Fine Chemicals, India. Graphite powder was obtained from Sisco Research Laboratories (SRL). Sulfuric acid (H2SO4), ferric chloride hexahydrate (FeCl3·6H2O), sodium nitrate (NaNO3), and aqueous ammonia solution (25%) were purchased from Merck. All solutions for experiments were prepared using deionised water.

2.2. Synthesis of rGO via the chemical reduction method

Graphene oxide (GO) was synthesised from graphite using modified Hummer's method as described in.35,36 For the preparation of reduced graphene oxide (rGO), 320 mg of GO was dispersed in 120 mL of deionised water and sonicated to achieve a uniform suspension. Subsequently, 32 µL of hydrazine hydrate was added, and the mixture was heated at 180 °C under hydrothermal conditions for 18 hours. During this process, oxygen-containing groups were removed, restoring the sp2 carbon network and resulting in a colour change from brown to black, which confirmed the formation of rGO. The resulting product was purified by centrifugation, dried at 80 °C, and ground into a powder to obtain rGO.

2.3. Synthesis of SnFe2O4–rGO via co-precipitation method

The nanocomposite was prepared via a simple co-precipitation method.37,38 About 100 mg of powdered rGO was well dispersed in 0.1 L of distilled water. FeCl3·6H2O of 1.2 g and SnCl2·2H2O of 0.8 g were added to the rGO solution and allowed to dissolve completely. This reaction mixture was heated to 80 °C, followed by the addition of 2 M of ammonium hydroxide (NH4OH) to attain a pH of 10, which facilitates the formation of precipitate in the form of hydroxides. Afterward, the formed precipitate was rinsed several times with a deionized water-ethanol mixture, dried at 80 °C, and calcined for 3 hours at 700 °C, followed by grinding to obtain SnFe2O4–rGO.

2.4. Photocatalytic degradation of MB

The photocatalytic degradation efficiency of SnFe2O4–rGO was evaluated using MB degradation under simulated visible-light irradiation. Photocatalytic experiments were conducted under various conditions by preparing reaction mixtures containing MB at different concentrations (100 ppm stock solutions), varying pH values, and different catalyst loadings. Each reaction mixture was stirred in the dark for 30 minutes before light irradiation to establish adsorption–desorption equilibrium between the catalyst and MB. Prepared solutions were transferred to quartz tubes and placed in the photoreactor for a particular time. About 1 mL aliquots were collected at regular intervals (15 minutes), centrifuged, and subjected to UV-visible spectroscopy analysis. The change in absorbance value at 665 nm was monitored throughout the reaction. From UV analysis data, the percentage of catalytic efficiency was then calculated using eqn (1). η is the SnFe2O4–rGO photocatalytic efficiency in percentage, C0 is the initial MB concentration before light irradiation, and Cf represents the concentration of MB at the end of the reaction.

2.4. 1

2.5. Computational methods

Density functional theory (DFT) calculations were performed utilizing the Gaussian 16 program package.39 The molecular geometries of graphene oxide and reduced graphene oxide (rGO) were optimized at the B3LYP- D3(BJ)/6-311++G(d,p) level of theory without any applying any symmetry constraints.40,41 The basis set used was 6-311++G (d,p), a triple-split-valence Pople-type basis set augmented with diffuse (++) and polarization functions (d,p).39 It better describes electron distribution in extended π-conjugated systems. Grimme's D3 correction with Becke–Johnson damping [D3(BJ)] was employed to account for dispersion interactions at long ranges that play a significant part in both π–π stacking and interlayer interactions of the graphene derived systems.42,43 Following the geometry optimization of graphene oxide (GO) and reduced graphene oxide (rGO), subsequent DFT calculations were performed on the SnFe2O4–rGO composite at the same level of theory. In this case, a mixed basis set was implemented using the “Gen” keyword. Specifically, the 6-311++G(d,p) basis set was employed to describe the non-metal atoms, while the LANL2DZ basis set was used to describe the metal atoms (Fe and Sn). These methodologies are common in studies involving hybrid materials that contain elements from both the main-group and transition metal categories and help achieve an equilibrium between computational accuracy and cost while not sacrificing structural and electronic properties.44,45

2.6. Instrumentation and characterisation of materials

Several advanced techniques were employed to comprehensively characterise the synthesised photocatalysts. Powder X-ray Diffraction (p-XRD) was used to determine crystalline structure, while Thermogravimetric Analysis (TGA) measured thermal stability and decomposition. Optical properties, including absorption and bandgap, were assessed using UV-vis spectroscopy and Tauc plots. Morphology and elemental distribution were examined using Field Emission Scanning Electron Microscopy (FE-SEM) coupled with Energy-Dispersive X-ray Spectroscopy (EDX). X-ray Photoelectron Spectroscopy (XPS) provided information on surface composition and oxidation states. Selected-Area Electron Diffraction (SAED) and High-Resolution Transmission Electron Microscopy (HR-TEM) offered further insights into microstructure. The Brunauer–Emmett–Teller (BET) method was applied to measure surface area, pore volume and pore size. Raman spectroscopy was utilised to investigate structural defects in GO and rGO. The point of zero charge (PZC) and zeta potential were measured to evaluate surface charge and colloidal stability in aqueous media. Electrochemical studies were conducted to explore the redox properties of the catalysts. Photocatalytic activity under visible light was tested in a photoreactor, and degradation efficiency was monitored using UV-vis spectrophotometer.

3. Results and discussions

3.1. Catalyst characterizations

Powder X-ray diffraction (p-XRD) analysis was used to determine the phase purity and crystallinity of the synthesised materials. The diffraction pattern of GO Fig. S1, showed a peak at 10.2°, confirming graphite's oxidation and exfoliation. Following chemical reduction, this peak shifted to 24.4°, indicating conversion to rGO. As shown in Fig. 1, both SnFe2O4 and SnFe2O4–rGO exhibited sharp diffraction peaks, indicating high crystallinity. Comparison with the JCPDS database (01-071-0695) confirmed that SnFe2O4 is a pure inverse spinel, with dominant reflections indexed to the (220), (222), (511), (440), and (442) planes. In the SnFe2O4–rGO nanocomposite, SnFe2O4 peaks shifted slightly, but no new peaks appeared, indicating the spinel framework remained stable after rGO incorporation and calcination.46 The rGO diffraction peak appeared near 25°, and a minor red shift in nanohybrid peaks could be due to changes in crystallinity and particle size during calcination.

Fig. 1. p-XRD patterns of SnFe2O4 and SnFe2O4–rGO nanohybrid, highlighting phase formation and crystallinity enhancement.

Fig. 1

Morphological and structural characteristics of the synthesized nanocatalysts were evaluated using Field Emission Scanning Electron Microscopy (FESEM), a high-resolution imaging technique that provides detailed surface information at the nanoscale. In Fig. 2, GO (graphene oxide) displays a wrinkled, layered structure, indicating complete oxidation of graphite to graphene oxide. After hydrazine hydrate reduction, the sheets appear disordered and crumpled, confirming the formation of reduced graphene oxide (rGO). The FESEM micrograph of SnFe2O4 (tin ferrite) shows randomly distributed spherical structures clustered between 50–100 nm.47 In the nanocomposite material, micrographs clearly show uniform anchoring of these spherical particles onto layered sheets, implying successful integration of SnFe2O4 nanoparticles and rGO. The optimized morphology enhances the synergistic (combined) properties of the hybrid material. Along with FESEM, EDX (Energy Dispersive X-ray) spectroscopy verified the elemental composition and purity, as shown in Fig. 3. The EDX spectrum of the SnFe2O4–rGO nanocomposite confirmed tin (Sn), iron (Fe), oxygen (O), and carbon (C), with no extra peaks, ruling out impurities. The EDX profile of rGO showed a significant decrease in oxygen relative to GO, providing direct elemental evidence of successful chemical reduction. These results, in agreement with p-XRD (powder X-ray diffraction) and XPS (X-ray photoelectron spectroscopy) analyses, confirm the controlled composition and high purity of the synthesized nanocatalysts.

Fig. 2. FESEM images of (a) GO (b) rGO, (c) SnFe2O4, and (d) SnFe2O4–rGO highlighting their distinct surface morphologies and nanostructures.

Fig. 2

Fig. 3. EDX spectra of (a) GO (b) rGO (c) SnFe2O4 and (d) SnFe2O4–rGO nanohybrid, illustrating the elemental composition and confirming the presence of key constituent elements in each sample.

Fig. 3

To assess the optical properties and band gaps of the synthesised nano catalysts, ultraviolet-visible diffuse reflectance spectroscopy (UV-DRS) was used. The DRS spectrum of rGO (Fig. S2a) shows a sharp absorption at 280 nm, indicating sensitivity to UV light. Pristine SnFe2O4 exhibits strong absorption across the visible region (∼450–700 nm) due to its narrower band gap. For the SnFe2O4–rGO nanocomposite, the absorption edge (Fig. 4a) is red-shifted, indicating a strong interaction between SnFe2O4 and rGO. Combined with rGO's superior conductivity and SnFe2O4 visible-light response, this leads to enhanced photo absorption across the UV-visible range. Optical band gaps (Eg) calculated from Tauc plots are 2.95 eV, 1.6 eV, and 1.50 eV for rGO, SnFe2O4, and SnFe2O4–rGO, respectively (Fig. S2b and 4b). The reduced band gap in the nanohybrids allows broader visible-light absorption and more efficient separation of charge carriers, explaining their enhanced photocatalytic activity.

Fig. 4. (a) UV-DRS spectra (b) Tauc's plot of SnFe2O4, SnFe2O4–rGO for optical band gap determination.

Fig. 4

X-ray photoelectron spectroscopy (XPS) identified the elemental oxidation states in the SnFe2O4–rGO nanocomposite. Fig. 5 shows the XPS spectra for each element and a survey spectrum of the oxidation states. In the C 1s spectrum, two peaks at 284.6 eV and 288.1 eV correspond to C–C/C Created by potrace 1.16, written by Peter Selinger 2001-2019 C bonds and O–C Created by potrace 1.16, written by Peter Selinger 2001-2019 O bonds respectively, confirming the incorporation of reduced graphene oxide (rGO) into SnFe2O4. The Fe 2p spectrum shows main peaks at 710.9 eV (Fe 2p3/2) and 724.4 eV (Fe 2p1/2), confirming Fe3+ ions. A satellite peak indicates high-spin Fe3+.48 The Sn 3d spectrum displays peaks at 485.9 eV (Sn 3d5/2) and 494.3 eV (Sn 3d3/2), suggesting tin is mainly in the Sn2+ oxidation state.45 These values are consistent with Sn2+ species reported for Fe–Sn oxide systems.46 Sn2+ facilitates charge transfer and enhances photocatalytic reactions.49 The presence of Sn2+ may contribute to the electronic interactions withing the SnFe2O4-based composite. In a related SnFe2O4/α-Fe2O3 heterojunction, Jo and research group reported that the intimate interface promoted Z-scheme charge transfer and enhanced charge separation, thereby improving photocatalytic CO2 reduction.50 Together, the survey and high-resolution spectra confirm the successful synthesis of the SnFe2O4–rGO heterojunction.

Fig. 5. XPS spectra (a) C 1s (b) O 1s (c) Sn 3d (d) Fe 2p and (e) survey spectrum confirming elemental composition and oxidation states in the SnFe2O4–rGO nanohybrid.

Fig. 5

Brunauer–Emmett–Teller surface area analysis revealed that the SnFe2O4–rGO nanocomposite exhibits a mesoporous structure with a high specific surface area, both of which are critical for its enhanced photocatalytic efficiency. Pure rGO exhibited a type IV nitrogen adsorption–desorption isotherm with an H4 hysteresis loop and a specific surface area of 266.55 m2 g−1, as shown in Fig. 6. This is attributed to its unique layered structure, including folds and wrinkles that prevent sheet restacking.50 In contrast, the nanocomposite showed a reduced surface area of 83.21 m2 g−1 due to partial blocking of rGO sheets by SnFe2O4 nanoparticles; however, this remains sufficient for efficient catalytic activity. The isotherm also confirms a narrow, slit-shaped mesoporous network within the nanocomposite.51 Additionally, the Barrett–Joyner–Halenda (BJH) technique measured a pore diameter of 1.429 nm and a volume of 0.203 cc g−1, indicating mesoporosity that aids transport and diffusion of reactant molecules.52 Overall, the high surface area and mesoporous structure of SnFe2O4–rGO increase light absorption and reactant adsorption, accelerating photocatalytic performance.

Fig. 6. N2 adsorption–desorption isotherm of SnFe2O4–rGO nanocomposite depicting specific surface area, pore volume, and pore size distribution to characterise its porous structure.

Fig. 6

Thermogravimetric analysis (TGA), which measures changes in sample mass with temperature, and differential thermal analysis (DTA), which compares a sample's temperature change to a reference, were carried out to assess the stability of SnFe2O4–rGO at higher temperatures and to further determine the optimal calcination temperature (Fig. 7). Optimising the calcination temperature helps to ensure thorough thermal processing and aids understanding of material stability.53 Initially, the loss of weight under 100 °C corresponds to the removal of water and other volatile substances present on the SnFe2O4–rGO surface. A significant decrease in mass of about 18% between 150 °C and 450 °C is mainly due to the removal of oxygen-containing groups from rGO, releasing gases such as carbon monoxide (CO) and carbon dioxide (CO2), and the elimination of hydroxyl groups (–OH) from the SnFe2O4 component. After 550 °C, a steady decline in mass is observed, which corresponds to the combustion and partial decomposition of the SnFe2O4–rGO structure.54 A sharp curve around 650 °C indicates the onset of thermal stabilization with zero weight loss. Based on these observations, the calcination temperature was set at 700 °C, providing a reliable basis for further thermal analysis.

Fig. 7. TGA-DTA plot of the SnFe2O4–rGO, illustrating its thermal stability and decomposition behaviour.

Fig. 7

The DTA spectrum provides further insight into the material's thermal behaviour. The sharp endothermic peak at 78 °C corresponds to the vaporisation of physically adsorbed water molecules and volatile molecules. A broad peak from 80 °C to 750 °C indicates various thermal breakdowns and overlapping of oxygen-containing and hydroxyl functional groups. This could also lead to various endothermic and exothermic reactions and determine the structural and chemical changes within SnFe2O4–rGO. In short, the DTA results support the TGA curve, which shows an initial desorption process followed by decomposition, structural rearrangements, and phase transitions as the temperature rises.

The electronic properties of nano catalysts for photocatalysis were investigated with photoluminescence (PL) and electrochemical impedance spectroscopy (EIS). During photocatalytic degradation, electron–hole pair recombination can reduce efficiency.55Fig. 8a shows that the PL spectrum of SnFe2O4–rGO is lower than that of pristine SnFe2O4, indicating a notable suppression of charge-carrier recombination. Charge-transfer properties were examined using EIS. As shown in Fig. 8b, the Nyquist plot shows a smaller arc for SnFe2O4–rGO than for SnFe2O4, indicating lower charge-transfer resistance and improved electron mobility within the composite.56 Overall, PL and EIS findings confirm that adding rGO to SnFe2O4 is key to suppressing charge-carrier recombination and promoting efficient charge transport, thereby enhancing the photocatalytic performance of SnFe2O4–rGO.

Fig. 8. (a) PL spectra revealing charge carrier recombination and defect states (b) Nyquist plots illustrating charge transfer resistance and electrical conductivity of the samples.

Fig. 8

The surface-charge characteristics of SnFe2O4 and SnFe2O4–rGO were examined using PZC and zeta-potential measurements. The PZC indicates the pH at which the net surface charge approaches zero and provides information on the pH-dependent surface chemistry. The shift in PZC after rGO incorporation suggests a change in the surface properties of SnFe2O4, which may influence dye adsorption and interfacial reactions. The zeta potentials of SnFe2O4 and SnFe2O4–rGO were −27.3 and −22.6 mV, respectively, indicating a change in the surface electrokinetic properties after rGO incorporation. Although both samples exhibited negative zeta potentials under the measured conditions, the less negative value of the nanohybrid suggests a modified interfacial charge environment. These changes may contribute to the adsorption and charge-transfer behaviour of the photocatalyst during MB degradation.57 Zeta potential measurements corroborate these findings, as depicted in Fig. 9b. Pure SnFe2O4 exhibits a zeta potential of −27.3 mV, while the SnFe2O4–rGO nanohybrid presents a slightly less negative value of −22.6 mV, indicating that rGO modifies the surface charge properties. Although both samples retain an overall negative surface charge, the reduced magnitude in the hybrid material may influence particle dispersibility and adsorption dynamics differently than in the pure material.58,59 Collectively, the combined PZC and EIS results demonstrate that the incorporation of rGO into SnFe2O4 significantly enhances the surface and colloidal properties of SnFe2O4–rGO, thereby promoting interactions that can improve photocatalytic performance.

Fig. 9. (a) PZC plots and (b) zeta potential plots of SnFe2O4 and SnFe2O4–rGO showing the effect of rGO on surface charge and stability.

Fig. 9

3.2. Photocatalytic activity of SnFe2O4–rGO for MB degradation

The photocatalytic performance of the SnFe2O4–rGO nanohybrid was assessed via methylene blue (MB) degradation, as shown in Fig. 10a–c. To determine the effect of reduced graphene oxide (rGO), the activity of SnFe2O4–rGO was compared with that of pristine SnFe2O4 (Fig. S3a–c). The catalyst MB suspension was first kept in the dark to establish adsorption–desorption equilibrium, particularly considering the adsorption contribution of rGO. After equilibrium was reached, the suspension was irradiated, and the subsequent decrease in MB concentration was monitored. The concentration after dark equilibration was taken as (C0) for the kinetic analysis. Therefore, the observed MB removal during irradiation was evaluated separately from the initial adsorption step, and the decrease in the MB absorption band was not considered as direct evidence of complete degradation or mineralization. To maximize photocatalytic efficiency, key parameters such as initial dye concentration, catalyst dosage, and solution pH were varied individually while maintaining other factors constant.

Fig. 10. Photocatalytic degradation efficiency of MB using SnFe2O4–rGO under different conditions (a) concentration (b) pH (c) dosage (d) kinetics plot for rate constant determination.

Fig. 10

The experiments were conducted at a fixed catalyst dosage and pH. For both SnFe2O4 and SnFe2O4–rGO, degradation efficiency decreased as methylene blue (MB) concentration increased. Notably, higher efficiencies were observed at lower concentrations: specifically, 5 ppm for SnFe2O4 and 10 ppm for SnFe2O4–rGO. This improvement is likely due to the greater availability of active catalyst sites and reduced agglomeration of dye molecules, both of which facilitate adsorption. Moreover, enhanced light penetration at lower concentrations may also contribute to improved photocatalytic activity. Conversely, at higher dye concentrations (20 and 30 ppm), dye aggregation and limited access to catalyst active sites reduce light penetration, resulting in decreased degradation efficiency.60 Therefore, a dye concentration of 10 ppm for SnFe2O4–rGO was selected for subsequent experiments.

The effect of catalyst dosage was examined by varying the concentrations of SnFe2O4 and SnFe2O4–rGO from 0.2 to 1.4 mg mL−1, while maintaining constant optimized MB concentration and pH. Photocatalytic efficiency increased with catalyst dosage up to 1.0 mg mL−1, which can be attributed to a higher number of active sites and increased generation of reactive oxygen species (ROS), promoting MB degradation. However, above this optimal dosage, only marginal improvements were observed, likely due to particle agglomeration and excessive light scattering reducing effective catalyst activation. Therefore, 1.0 mg mL−1 was selected as the optimal catalyst dosage for SnFe2O4–rGO photocatalysis.

The influence of solution pH on the photocatalytic degradation of MB was evaluated over the pH range of 3–11 while keeping the initial dye concentration and catalyst dosage constant. The pH of the reaction medium can significantly affect the surface characteristics of SnFe2O4–rGO and, consequently, its interaction with the cationic MB molecules. The PZC measurements indicate that the surface charge of the photocatalyst varies with pH, which can influence dye adsorption and the availability of surface-active sites. Under acidic conditions, protonation of surface functional groups can result in a positively charged catalyst surface, which may cause electrostatic repulsion toward the cationic MB molecules. With increasing pH, deprotonation of surface groups can modify the surface charge and alter the adsorption behaviour of MB. However, the degradation efficiency is not determined by adsorption alone and can also depend on surface hydroxyl groups, charge-carrier separation, and the formation of reactive oxygen species. The highest degradation efficiency at pH 7 may therefore be attributed to a favourable balance between MB adsorption and the interfacial photocatalytic reactions occurring on the SnFe2O4–rGO surface. The observed pH dependence consequently reflects the combined influence of surface chemistry, dye–catalyst interactions, and photocatalytic charge-transfer processes rather than electrostatic interactions alone.

The photocatalytic performance of SnFe2O4 and SnFe2O4–rGO was further evaluated by analyzing the reaction kinetics to determine the rate constants. This parameter is essential for quantifying the maximum degradation achieved over time. The optimized conditions varied between the two catalysts. SnFe2O4–rGO exhibited 64.3% MB degradation at 10 ppm MB with a catalyst dosage of 1.0 mg mL−1, while pristine SnFe2O4 achieved 59.9% degradation at 5 ppm MB and 1.4 mg mL−1 catalyst. The higher efficiency of the composite under a higher dye concentration and lower catalyst dosage highlights its improved photocatalytic performance. Rate constants of 0.0916 min−1 for SnFe2O4 and 0.0982 min−1 for SnFe2O4–rGO were obtained, as shown in Fig. 10d. The higher rate constant observed for the nanohybrid suggests more rapid degradation. This is likely due to synergistic effects from reduced graphene oxide. The rGO enhances charge carrier separation, accelerates electron transport, and increases the available surface area for reaction. Although the difference in rate constants is modest, the results indicate that incorporating rGO into the SnFe2O4 matrix significantly accelerates MB degradation and improves overall photocatalytic performance. Table 1 summarizes the optimized factors and maximum efficiency achieved for the photocatalytic degradation of MB using both SnFe2O4 and SnFe2O4–rGO.

Table 1. Optimised parameters and photocatalytic degradation efficiencies of methylene blue (MB) using SnFe2O4 and SnFe2O4–rGO.

Photocatalyst Concentration (ppm) pH Catalyst dosage (mg mL−1) Efficiency (%) Rate constant (min−1)
SnFe2O4 5 9 1.4 59.9 0.0916
SnFe2O4–rGO 10 7 1 64.3 0.09820

Scavenging experiments were performed on SnFe2O4 and SnFe2O4–rGO to elucidate the photocatalytic degradation mechanism of methylene blue (MB).61 These studies are essential for identifying the key reactive species responsible for the degradation process. It is widely recognized that superoxide anion radicals (O2˙−), photogenerated holes (h+), and hydroxyl radicals (−OH) are the primary active species in photocatalytic reactions.62 In this study, specific quenchers were utilized to evaluate their effects on MB degradation with both SnFe2O4 and SnFe2O4–rGO. Fig. 11 shows that isopropyl alcohol (IPA) reduces degradation efficiency by scavenging hydroxyl radicals. Para-benzoquinone (p-BQ) neutralizes O2˙− radicals, and ethylenediaminetetraacetic acid (EDTA) is a hole scavenger. Both moderately inhibit MB degradation. These results indicate that hydroxyl radicals and photogenerated holes are the main contributors. Superoxide radicals play a secondary role in the photocatalytic degradation of MB by SnFe2O4–rGO. Identifying these active species clarifies the mechanism and enhances the nanohybrid's environmental applicability.

Fig. 11. Influence of various scavengers on the photocatalytic degradation performance of SnFe2O4 and SnFe2O4–rGO nanohybrids toward MB.

Fig. 11

The photocatalytic performance of the SnFe2O4–rGO heterojunction is dependent to the band edge potentials of each component, which dictate the movement and separation efficiency of photogenerated charge carriers vital for the degradation of methylene blue (MB). When the hybrid system is exposed to visible light, photons with energy equal to or greater than the bandgap of SnFe2O4 excite electrons from the valence band (VB) to the conduction band (CB), thereby creating electron–hole pairs. The band edge positions, valence band edge potential (EVB) and conduction band edge potential (ECB), were calculated using Mulliken electronegativity theory as per eqn (2) and (3).

EVB = X − Ee + 0.5 Eg 2
ECB = EVB − Eg 3

SnFe2O4 exhibits 1.56 eV, 1.623 eV values for EVB and ECB, respectively. Based on these band alignments, the transfer of photoexcited electrons between SnFe2O4 and rGO happens in the heterojunction, and a plausible mechanism is depicted in Fig. 12. The rGO effectively suppresses the recombination of electrons and holes, a common limitation in photocatalysts that reduces efficiency. Simultaneously, the holes left in the VB of SnFe2O4 possess strong oxidative potential and react with surface-adsorbed water or hydroxide ions to generate hydroxyl radicals, while the electrons transferred to rGO reduce dissolved oxygen molecules to form superoxide radicals. These reactive oxygen species (ROS) are highly potent, which can oxidise and break down the complex molecular structure of MB dye into less harmful substances. The MB degradation process, therefore, depends on this charge separation and the subsequent ROS-driven oxidation, which is supported by scavenger studies that identify the predominant reactive species responsible for the dye degradation.63,64 Based on the band-edge analysis and scavenging experiments, the following reactions are proposed as possible pathways.SnFe2O4–rGO + H2O → SnFe2O4–rGO + ˙OH + h+SnFe2O4–rGO + O2 → SnFe2O4–rGO + ˙O2˙O2 + h+ → H2Oh+ + OH → ˙OHO2 + e− → ˙O2−˙O2 + H2O → ˙OOH + OHH2O2 + ˙O2 → ˙OH + OH + O2˙OH + ˙O2 + h+ + MB → intermediates → CO2 + H2O

Fig. 12. Schematic illustration of the plausible photocatalytic degradation pathway of MB over the SnFe2O4–rGO heterojunction under visible-light irradiation.

Fig. 12

The reusability of the SnFe2O4 and SnFe2O4–rGO photocatalyst was systematically evaluated to assess its stability and practical applicability across multiple photocatalytic cycles. After each reaction, the catalyst was readily recovered by centrifugation and reused under identical operating conditions. Fig. 13 shows that the SnFe2O4–rGO composite maintained excellent stability. It retained a high level of photocatalytic activity, with only a slight reduction in efficiency after four consecutive cycles. This consistent performance is attributed to the robust structural integrity of the nanocomposite. The reduced graphene oxide framework effectively inhibits electron–hole recombination. SnFe2O4–rGO contains iron (Fe), which makes it magnetically responsive. As a result, the catalyst is easily separated and recycled using an external magnetic field, particularly in liquid-phase reactions.65,66 These results indicate that SnFe2O4–rGO is a highly stable, reusable, and efficient heterogeneous photocatalyst. This underscores its potential for practical wastewater treatment and environmental remediation applications (Fig. 14).

Fig. 13. Recyclability study illustrating sustained photocatalytic performance and stability over multiple degradation cycles of MB.

Fig. 13

Fig. 14. Geometries of graphene, graphene oxide, reduced graphene oxide (rGO), SnFe2O4, and SnFe2O4–rGO composites-1 and 2, obtained from computational calculations.

Fig. 14

3.3. Computational study

In recent studies, theoretical investigations have increasingly been employed to support and interpret experimental results, particularly in photocatalytic degradation.67 These theoretical calculations provide significant insights into structural properties, energy states and electronic density distributions at the atomic level. Frontier molecular orbital analysis was carried out and the HOMO–LUMO energy gap (ΔEH–L = energy of HOMO − energy of LUMO) was evaluated for graphene, rGO and SnFe2O4–rGO to understand the evolution of the electronic structure. The progressive narrowing and tuning of the HOMO–LUMO gap from graphene to rGO and further to SnFe2O4–rGO is correlated with enhanced charge separation and improved photocatalytic activity of the composite material.68 The HOMO–LUMO energy analysis was carried out to understand the effect of SnFe2O4 loading on the electronic properties of reduced graphene oxide (rGO). The calculated band gap of pristine graphene, graphene oxide, and rGO was found to be approximately 3.16–3.19 eV, indicating relatively poor charge-transport characteristics (Fig. 15) (Table 2).

Fig. 15. Pictorial representation of energy difference between the Highest Occupied Molecular Orbital (HOMO) and Lowest Unoccupied Molecular Orbitals (LUMO) of graphene, graphene oxide and reduced graphene oxide (rGO).

Fig. 15

Table 2. Comparison of energies for the frontier molecular orbital and global reactivity indices. All the values are given in eV.

Material E HOMO E LUMO E g IP EA χ η S µ ω N
Graphene −5.18 −2.01 3.19 5.18 2.01 3.6 1.59 0.31 −3.6 4.08 2.26
rGO −5.4 −2.22 3.17 5.4 2.22 3.81 1.59 0.31 −3.81 4.57 2.4
GO −5.54 −2.38 3.16 5.54 2.38 3.96 1.58 0.32 −3.96 4.96 2.51
SnFe2O4–rGO composite-1 −5.22 −4.8 0.42 5.22 4.8 5.01 0.21 2.38 −5.01 59.76 23.86
SnFe2O4–rGO composite-2 −5.2 −5.02 0.18 5.2 5.02 5.11 0.09 5.56 −5.11 145.1 56.78

However, upon formation the SnFe2O4–rGO composite has been found to have a significantly smaller energy gap than pure SnFe2O4. The HOMO–LUMO energy gaps (ΔEH–L) of the configurations were as follows: the SnFe2O4–rGO-2 configuration had an energy gap of 0.2 eV and the SnFe2O4–rGO-1 configuration exhibited an energy gap of 0.42 eV. The reduced energy gap suggests significant electronic interaction between rGO and SnFe2O4. This would allow for an easier activation of electrons into higher energy states and facilitate the movement of charge carriers. Therefore, it can be anticipated that the SnFe2O4–rGO nanocomposite will exhibit improved photocatalysis activity compared with SnFe2O4 alone. The composites show a significant decrease in chemical hardness from around 1.58–1.59 eV in graphene, GO, and rGO to 0.21 eV and 0.09 eV for composite-1 and composite-2, respectively. This decrease signifies a reduction in resistance to charge transfer, making it easier for electrons to move from one composite to another and enabling fast surface redox reactions. A similar observation is made for softness values, where graphene, GO and rGO show softness in the range of ∼0.31–0.32 eV, while the composites show significantly higher values of 2.38 eV and 5.56 eV. This signifies an increase in the electronic polarizability and conductivity, which makes it easier for the photogenerated charge carriers to move from one composite to another, thus reducing recombination (Fig. 16).

Fig. 16. Pictorial representation of energy difference between the Highest Occupied Molecular Orbital (HOMO) and Lowest Unoccupied Molecular Orbitals (LUMO) of two possible composites of reduced graphene oxide (rGO) and SnFe2O4 spinel.

Fig. 16

The electrophilicity index (ω) also shows a significant increase in the composites, which ranges from approximately 4.08–4.96 eV in graphene, GO, and rGO to 59.76 eV and 145.07 eV for composite-1 and 2. These exceptionally large values primarily originates from the very small calculated hardness values and therefore directly it cannot be interpreted as quantitative measures of intrinsic electron-accepting ability of the bulk composites. Instead, the observed relative trend in ω provides qualitative evidence for enhanced electron-accepting ability of the bulk composite. The maximum charge transfer parameter (N) also increases from around 2.26–2.51 eV in graphene-based systems to 23.86 and 56.78 eV in the composites. Overall, the rGO–SnFe2O4 nanocomposite is expected to exhibit improved photocatalytic performance due to efficient charge separation and suppressed electron–hole recombination. These findings support the experimental observation of enhanced photocatalytic degradation of methylene blue. Although the trend remains to be similar, yet we observed a finite difference between experimental bandgap and theoretical ΔEH–L values. This discrepancy arises because our computational study employed a finite small molecular cluster as a representative of the composite material and these cluster-model frontier-orbital energies i.e. ΔEH–L are distinct from experimental band gaps. In this context, the relative trend in ΔEH–L across the studied systems is more meaningful than its absolute magnitude, as it provides qualitative insight into their relative electronic properties. Additionally, discrepancy arises from intrinsic and methodological factors too. Experimentally in UV-DRS spectroscopy, we can determine the optical bandgap from photon absorption, which is influenced by the material's electronic structure and light-scattering effects. In SnFe2O4–rGO, these influential factors can cause band tailing and reduce absorption efficiency, thereby increasing the band gap. In DFT calculations, an idealized defect-free crystal structure at equilibrium is used. This may lower the energy gaps due to exchange-correlation functionals and the omission of lattice strain and interfacial charge transfer, which are facilitated by the introduction of rGO. Therefore, the comparatively higher bandgap observed in the UV-DRS results from experimental limitations, as indicated by DFT calculations. Defects and simplified assumptions.69,70

4. Summary

This study systematically investigated the synthesis, optimization, and application of SnFe2O4–rGO as a visible-light-activated photocatalyst for the degradation of methylene blue. The SnFe2O4–rGO composite demonstrated higher photocatalytic efficiency than its individual components. Variation in reaction parameters, such as dye concentration, catalyst dosage, and solution pH, resulted in high degradation rates and significant reusability. The interaction between SnFe2O4 and reduced graphene oxide enhanced charge carrier separation at the interface, reducing recombination losses, improving light absorption, and increasing the catalyst's effective surface area. The scavenging results indicate that hydroxyl radicals and photogenerated holes are the major reactive species involved in MB degradation, with superoxide radicals contributing to a lesser extent. UV-vis spectroscopy confirmed efficient electron transfer and enabled monitoring of the formation of degradation products. Although experiments were conducted under controlled laboratory conditions with a model pollutant, the findings establish a basis for future research on water treatment involving mixed contaminants and catalyst stability. These results contribute to the advancement of sustainable photocatalytic materials for environmental remediation.

Conflicts of interest

The authors declare no competing interests.

Supplementary Material

RA-OLF-D6RA07029A-s001

Data availability

The datasets generated and/or analysed during the current study are available in the manuscript. Additional data or computational details can be made available by the corresponding author upon reasonable request.

Supplementary information (SI): the Cartesian coordinates for graphene, graphene oxide (GO), reduced graphene oxide (rGO), SnFe2O4, and the SnFe2O4–rGO composites (1 and 2). See DOI: https://doi.org/10.1039/d6ra07029a.

References

  1. Morshedy A. S. El-Fawal E. M. Zaki T. El-Zahhar A. A. Alghamdi M. M. El Naggar A. M. A review on heterogeneous photocatalytic materials: mechanism, perspectives, and environmental and energy sustainability applications. Inorg. Chem. Commun. 2024;163:112307. doi: 10.1016/j.inoche.2024.112307. [DOI] [Google Scholar]
  2. Ameen S. Fatima R. Kadhem A. A. Abbas T. Khan M. A. Abbas A. Hussain I. Bano N. Faraji Rad Z. Bilal A. S. Enhanced photocatalytic degradation of methylene blue using aluminum and cerium co-doped ZnO nanocomposite. Int. J. Environ. Sci. Technol. 2025;22(16):16549–16558. doi: 10.1007/s13762-025-06683-z. [DOI] [Google Scholar]
  3. Acedo-Mendoza A. G. Infantes-Molina A. Vargas-Hernández D. Chávez-Sánchez C. A. Rodríguez-Castellón E. Tánori-Córdova J. C. Photodegradation of methylene blue and methyl orange with CuO supported on ZnO photocatalysts: The effect of copper loading and reaction temperature. Mater. Sci. Semicond. Process. 2020;119:105257. doi: 10.1016/j.mssp.2020.105257. [DOI] [Google Scholar]
  4. Khan I. Saeed K. Zekker I. Zhang B. Hendi A. H. Ashfaq A. Ahmad S. Zada N. Hanif A. Shah L. A. Shah T. Review on methylene blue: its properties, uses, toxicity and photodegradation. Water. 2022;14(2):242. doi: 10.3390/w14020242. [DOI] [Google Scholar]
  5. Lanjwani M. F. Tuzen M. Khuhawar M. Y. Saleh T. A. Trends in photocatalytic degradation of organic dye pollutants using nanoparticles: a review. Inorg. Chem. Commun. 2024;159:111613. doi: 10.1016/j.inoche.2023.111613. [DOI] [Google Scholar]
  6. Samsami S. Mohamadizaniani M. Sarrafzadeh M. H. Rene E. R. Firoozbahr M. Recent advances in the treatment of dye-containing wastewater from textile industries: overview and perspectives. Process Saf. Environ. Prot. 2020;143:138–163. doi: 10.1016/j.psep.2020.05.034. [DOI] [Google Scholar]
  7. Kalaycıoğlu Z. Özuğur Uysal B. Pekcan O. Erim F. B. Efficient photocatalytic degradation of methylene blue dye from aqueous solution with cerium oxide nanoparticles and graphene oxide-doped polyacrylamide. ACS Omega. 2023;8(14):13004–13015. doi: 10.1021/acsomega.3c00198. [DOI] [PMC free article] [PubMed] [Google Scholar]
  8. Bhatia D. Sharma N. R. Singh J. Kanwar R. S. Biological methods for textile dye removal from wastewater: a review. Crit. Rev. Environ. Sci. Technol. 2017;47(19):1836–1876. doi: 10.1080/10643389.2017.1393263. [DOI] [Google Scholar]
  9. Sirirerkratana K. Kemacheevakul P. Chuangchote S. Color removal from wastewater by photocatalytic process using titanium dioxide-coated glass, ceramic tile, and stainless steel sheets. J. Cleaner Prod. 2019;215:123–130. doi: 10.1016/j.jclepro.2019.01.037. [DOI] [Google Scholar]
  10. Paździor K. Bilińska L. Ledakowicz S. A review of the existing and emerging technologies in the combination of AOPs and biological processes in industrial textile wastewater treatment. Chem. Eng. J. 2019;376:120597. doi: 10.1016/j.cej.2018.12.057. [DOI] [Google Scholar]
  11. Chen D. Cheng Y. Zhou N. Chen P. Wang Y. Li K. Huo S. Cheng P. Peng P. Zhang R. Wang L. Photocatalytic degradation of organic pollutants using TiO2-based photocatalysts: a review. J. Cleaner Prod. 2020;268:121725. doi: 10.1016/j.jclepro.2020.121725. [DOI] [Google Scholar]
  12. Shakoor M. H. Shakoor M. B. Jilani A. Ahmed T. Rizwan M. Dustgeer M. R. Iqbal J. Zahid M. Yong J. W. Enhancing the photocatalytic degradation of methylene blue with graphene oxide-encapsulated g-C3N4/ZnO ternary composites. ACS Omega. 2024;9(14):16187. doi: 10.1021/acsomega.3c10172. [DOI] [PMC free article] [PubMed] [Google Scholar]
  13. Zhang H. Cao Y. Wang S. Tang Y. Tian L. Cai W. Wei Z. Wu Z. Zhu Y. Guo Q. Photocatalytic removal of ammonia nitrogen from water: investigations and challenges for enhanced activity. Environ. Sci. Pollut. Res. 2024;31(29):41824–41843. doi: 10.1007/s11356-024-33891-w. [DOI] [PubMed] [Google Scholar]
  14. Mottammal D. Thomas S. A. Cherusseri J. Kumar A. Rajendran D. N. Photocatalytic Degradation of Methylene Blue: Performance, Mechanism, and Perspectives. Top. Catal. 2026;69(8):1252–1292. doi: 10.1007/s11244-025-02234-5. [DOI] [Google Scholar]
  15. Ebanezar John A. Mishra D. Thankaraj Salammal S. Akram Khan M. Factors that enhance the efficiency of TiO2 based heterogeneous photocatalyst for its application in waste water treatment containing organic dye. Sustainable Water Resour. Manag. 2024;10(3):105. doi: 10.1007/s40899-024-01074-7. [DOI] [Google Scholar]
  16. Gouadria S. Al-Sehemi A. G. Manzoor S. Abdullah M. Abid A. G. Raza N. Panina L. V. Sayyed M. I. Tishkevich D. I. Trukhanov A. V. Design and preparation of novel LaFeO3/NiFe2O4 nanohybrid for highly efficient photodegradation of methylene blue dye under visible light illumination. J. Photochem. Photobiol., A. 2024;448:115305. doi: 10.1016/j.jphotochem.2023.115305. [DOI] [Google Scholar]
  17. Sanchez-Lievanos K. R. Sun T. Gendrich E. A. Knowles K. E. Surface adsorption and photoinduced degradation: a study of spinel ferrite nanomaterials for removal of a model organic pollutant from water. Chem. Mater. 2024;36(9):3981. doi: 10.1021/acs.chemmater.3c01986. [DOI] [PMC free article] [PubMed] [Google Scholar]
  18. Kirankumar V. S. Sumathi S. A review on photodegradation of organic pollutants using spinel oxide. Mater. Today Chem. 2020;18:100355. doi: 10.1016/j.mtchem.2020.100355. [DOI] [Google Scholar]
  19. Parastar Gharehlar M. Sheshmani S. Nikmaram F. R. Doroudi Z. Synergistic potential in spinel ferrite MFe2O4 (M = Co, Ni) nanoparticles-mediated graphene oxide: Structural aspects, photocatalytic, and kinetic studies. Sci. Rep. 2024;14(1):4625. doi: 10.1038/s41598-024-55452-4. [DOI] [PMC free article] [PubMed] [Google Scholar]
  20. Yin X. Li H. Yuan R. Jiao Y. Lu J. Templated synthesis of spinel cobaltite MCo2O4 (M = Ni, Co and Mn) hierarchical nanofibers for high performance supercapacitors. J. Mater. 2021;7(4):858–868. [Google Scholar]
  21. Chai H. Zhu J. Feng Y. Liang F. Wu Q. Ju Z. Huang L. Wang W. Capillarity enabled large-array liquid metal electrodes for compact and high-throughput dielectrophoretic microfluidics. Adv. Mater. 2024;36(21):2310212. doi: 10.1002/adma.202310212. [DOI] [PubMed] [Google Scholar]
  22. Zhao T. Zheng Y. Meng Y. Huang X. Chen S. Chang L. Shen J. ZnFe2O4 nanoparticles embedded dispersedly inside 3D porous carbon framework as advanced anode materials of Li-ion batteries. J. Alloys Compd. 2022;913:165279. doi: 10.1016/j.jallcom.2022.165279. [DOI] [Google Scholar]
  23. Bashal A. H. Hefnawy M. A. Ahmed H. A. El-Atawy M. A. Pashameah R. A. Medany S. S. Green synthesis of NiFe2O4 nano-spinel oxide-decorated carbon nanotubes for efficient capacitive performance—Effect of electrolyte concentration. Nanomaterials. 2023;13(19):2643. doi: 10.3390/nano13192643. [DOI] [PMC free article] [PubMed] [Google Scholar]
  24. El Moussaoui H. Mahfoud T. Habouti S. El Maalam K. Ali M. B. Hamedoun M. Mounkachi O. Masrour R. Hlil E. K. Benyoussef A. Synthesis and magnetic properties of tin spinel ferrites doped manganese. J. Magn. Magn. Mater. 2016;405:181–186. doi: 10.1016/j.jmmm.2015.12.059. [DOI] [Google Scholar]
  25. Liu Q. Luo Y. Yang S. Xiong Y. Wang R. Fu X. Zhang R. Hu S. Bao X. Xu C. Transfer-free in situ synthesis of high-performance polybenzimidazole grafted graphene oxide-based proton exchange membrane for high-temperature proton exchange membrane fuel cells. J. Power Sources. 2023;559:232666. doi: 10.1016/j.jpowsour.2023.232666. [DOI] [Google Scholar]
  26. Zheng Y. Shen Y. Guo J. Li J. Wang J. Ning D. Liu Y. Huang Y. Tang Y. Deng Y. Yan H. Recent advances in solid-state lithium batteries based on anode engineering. Nano Res. Energy. 2024;3(3):e9120118. doi: 10.26599/NRE.2024.9120118. [DOI] [Google Scholar]
  27. Chen D. Wang Q. Wang R. Shen G. Ternary oxide nanostructured materials for supercapacitors: a review. J. Mater. Chem. A. 2015;3(19):10158–10173. doi: 10.1039/C4TA06923D. [DOI] [Google Scholar]
  28. Bhatia D. Sharma N. R. Singh J. Kanwar R. S. Biological methods for textile dye removal from wastewater: a review. Crit. Rev. Environ. Sci. Technol. 2017;47(19):1836–1876. doi: 10.1080/10643389.2017.1393263. [DOI] [Google Scholar]
  29. Saini S. Chand P. Joshi A. Biomass derived carbon for supercapacitor applications. J. Energy Storage. 2021;39:102646. doi: 10.1016/j.est.2021.102646. [DOI] [Google Scholar]
  30. Lee K. T. Lu S. Y. A cost-effective, stable, magnetically recyclable photocatalyst of ultra-high organic pollutant degradation efficiency: SnFe2O4 nanocrystals from a carrier solvent assisted interfacial reaction process. J. Mater. Chem. A. 2015;3(23):12259–12267. doi: 10.1039/C5TA02278A. [DOI] [Google Scholar]
  31. Jo W. K. Moru S. Tonda S. Magnetically responsive SnFe2O4/g-C3N4 hybrid photocatalysts with remarkable visible-light-induced performance for degradation of environmentally hazardous substances and sustainable hydrogen production. Appl. Surf. Sci. 2020;506:144939. doi: 10.1016/j.apsusc.2019.144939. [DOI] [Google Scholar]
  32. Reddy D. H. Yun Y. S. Spinel ferrite magnetic adsorbents: alternative future materials for water purification? Coord. Chem. Rev. 2016;315:90–111. doi: 10.1016/j.ccr.2016.01.012. [DOI] [Google Scholar]
  33. Singh P. K. Kuo K. Y. Lee J. T. Hsiao P. H. Juan J. C. Duong H. P. Chen C. Y. Synergistic absorbents based on SnFe2O4@ZnO nanoparticles decorated with reduced graphene oxide for highly efficient dye adsorption at room temperature. RSC Adv. 2021;11(29):17840–17848. doi: 10.1039/D1RA02317A. [DOI] [PMC free article] [PubMed] [Google Scholar]
  34. Fan W. Gao W. Zhang C. Tjiu W. W. Pan J. Liu T. Hybridization of graphene sheets and carbon-coated Fe3O4 nanoparticles as a synergistic adsorbent of organic dyes. J. Mater. Chem. 2012;22(48):25108–25115. doi: 10.1039/C2JM35609K. [DOI] [Google Scholar]
  35. Narayanan V. Mandal B. K. Type-II ternary Bi2WO6/rGO/SnFe2O4 heterojunction nanocomposites and their photocatalytic efficiency towards 4-nitrophenol reduction. RSC Adv. 2023;13(32):22616–22629. doi: 10.1039/D3RA03647B. [DOI] [PMC free article] [PubMed] [Google Scholar]
  36. Elmoussaoui H. Hamedoun M. Mounkachi O. Benyoussef A. Masrour R. Hlil E. K. New results on magnetic properties of tin-ferrite nanoparticles. J. Supercond. Novel Magn. 2012;25(6):1995–2002. doi: 10.1007/s10948-012-1547-8. [DOI] [Google Scholar]
  37. Narayanan V. Mandal B. K. SnMn2O4-rGO: a mixed spinel on reduced graphene oxide as binary heterojunction for light induced oxidative degradation and reduction of environmental contaminants. Mater. Today Commun. 2025;44:111906. doi: 10.1016/j.mtcomm.2025.111906. [DOI] [Google Scholar]
  38. Narayanan V. Mandal B. K. Ragupathy G. Porous SnCo2O4-rGO nanohybrids for visible-light photocatalytic degradation of methylene blue and 4-nitrophenol reduction. Sci. Rep. 2026;16:18568. doi: 10.1038/s41598-026-40727-9. [DOI] [PMC free article] [PubMed] [Google Scholar]
  39. Frisch M. J., Trucks G. W., Schlegel H. B., Scuseria G. E., Robb M., Cheeseman J. R., Scalmani G., Barone V. P., Petersson G. A., Nakatsuji H. J. and Li X., Gaussian 16, Revision C. 01, Gaussian. Inc., Wallingford CT, 2016 [Google Scholar]
  40. Becke A. D. Density-functional thermochemistry. III. The role of exact exchange. J. Chem. Phys. 1993;98(7):5648–5652. doi: 10.1063/1.464913. [DOI] [Google Scholar]
  41. Lee C. Yang W. Parr R. G. Development of the Colle-Salvetti correlation-energy formula into a functional of the electron density. Phys. Rev. B:Condens. Matter Mater. Phys. 1988;37(2):785. doi: 10.1103/PhysRevB.37.785. [DOI] [PubMed] [Google Scholar]
  42. Krishnan R. B. Binkley J. S. Seeger R. Pople J. A. Self-consistent molecular orbital methods. XX. A basis set for correlated wave functions. J. Chem. Phys. 1980;72(1):650–654. doi: 10.1063/1.438955. [DOI] [Google Scholar]
  43. Grimme S. Antony J. Ehrlich S. Krieg H. A consistent and accurate ab initio parametrization of density functional dispersion correction (DFT-D) for the 94 elements H-Pu. J. Chem. Phys. 2010;132(15):154104. doi: 10.1063/1.3382344. [DOI] [PubMed] [Google Scholar]
  44. Anderson C. L. Zhang T. Qi M. Chen Z. Yang C. Teat S. J. Settineri N. S. Dailing E. A. Garzón-Ruiz A. Navarro A. Lv Y. Exceptional electron-rich heteroaromatic pentacycle for ultralow band gap conjugated polymers and photothermal therapy. J. Am. Chem. Soc. 2023;145(9):5474–5485. doi: 10.1021/jacs.3c00036. [DOI] [PubMed] [Google Scholar]
  45. Sowa J. K. Cadena D. M. Mehmood A. Levine B. G. Roberts S. T. Rossky P. J. IR Spectroscopy of carboxylate-passivated semiconducting nanocrystals: simulation and experiment. J. Phys. Chem. C. 2024;128(21):8724–8731. doi: 10.1021/acs.jpcc.4c01988. [DOI] [Google Scholar]
  46. Elmoussaoui H. Hamedoun M. Mounkachi O. Benyoussef A. Masrour R. Hlil E. K. New results on magnetic properties of tin-ferrite nanoparticles. J. Supercond. Novel Magn. 2012;25(6):1995–2002. doi: 10.1007/s10948-012-1547-8. [DOI] [Google Scholar]
  47. Jia Y. Wang Q. Zhang W. Kang M. Bae J. S. Liu C. Octahedron-shaped SnFe2O4 for boosting photocatalytic degradation and CO2 reduction. J. Alloys Compd. 2021;889:161737. doi: 10.1016/j.jallcom.2021.161737. [DOI] [Google Scholar]
  48. Liu X. Zhang J. Guo X. Wang S. Wu S. Core–shell α-Fe2O3@SnO2/Au hybrid structures and their enhanced gas sensing properties. RSC Adv. 2012;2(4):1650–1655. doi: 10.1039/C1RA00811K. [DOI] [Google Scholar]
  49. Luo H. Liang L. Y. Cao H. T. Liu Z. M. Zhuge F. Structural, chemical, optical, and electrical evolution of SnOx films deposited by reactive rf magnetron sputtering. ACS Appl. Mater. Interfaces. 2012;4(10):5673–5677. doi: 10.1021/am301601s. [DOI] [PubMed] [Google Scholar]
  50. Jo W. K. Kumar S. Eslava S. Tonda S. Construction of Bi2WO6/RGO/g-C3N4 2D/2D/2D hybrid Z-scheme heterojunctions with large interfacial contact area for efficient charge separation and high-performance photoreduction of CO2 and H2O into solar fuels. Appl. Catal., B. 2018;239:586–598. doi: 10.1016/j.apcatb.2018.08.056. [DOI] [Google Scholar]
  51. Murugesan P. Narayanan S. Manickam M. Murugesan P. K. Subbiah R. A direct Z-scheme plasmonic AgCl@g-C3N4 heterojunction photocatalyst with superior visible light CO2 reduction in aqueous medium. Appl. Surf. Sci. 2018;450:516–526. doi: 10.1016/j.apsusc.2018.04.111. [DOI] [Google Scholar]
  52. Li F. T. Xue Y. B. Li B. Hao Y. J. Wang X. J. Liu R. H. Zhao J. Precipitation synthesis of mesoporous photoactive Al2O3 for constructing g-C3N4-based heterojunctions with enhanced photocatalytic activity. Ind. Eng. Chem. Res. 2014;53(50):19540–19549. doi: 10.1021/ie5036258. [DOI] [Google Scholar]
  53. Liu Y. Liu H. Zhou H. Li T. Zhang L. A Z-scheme mechanism of N-ZnO/g-C3N4 for enhanced H2 evolution and photocatalytic degradation. Appl. Surf. Sci. 2019;466:133–140. doi: 10.1016/j.apsusc.2018.10.027. [DOI] [Google Scholar]
  54. Lu L. Wang G. Zou M. Wang J. Li J. Effects of calcining temperature on formation of hierarchical TiO2/g-C3N4 hybrids as an effective Z-scheme heterojunction photocatalyst. Appl. Surf. Sci. 2018;441:1012–1023. doi: 10.1016/j.apsusc.2018.02.080. [DOI] [Google Scholar]
  55. El Desouky F. G. Saadeldin M. M. Eisa W. H. Synergistic influence of SnFe2O4 on ZnSnO3 hybrid nanostructures and optimizations optical, photoluminescence, and magnetic properties for multifunction application. Surf. Interfaces. 2023;38:102749. doi: 10.1016/j.surfin.2023.102749. [DOI] [Google Scholar]
  56. Wei J. L. Wang Z. Y. Sun Y. H. Zhang G. L. Guan D. C. Nan J. M. The kinetics investigation of nitrogen/sulfur co-doped reduced graphene oxide@spinel SnFe2O4/Sn0.205Fe1.727O3 as high performance anode for lithium-ion batteries and its application in full cells. Electrochim. Acta. 2021;375:138026. doi: 10.1016/j.electacta.2021.138026. [DOI] [Google Scholar]
  57. Kosmulski M. Isoelectric points and points of zero charge of metal (hydr) oxides: 50 years after Parks' review. Adv. Colloid Interface Sci. 2016;238:1–61. doi: 10.1016/j.cis.2016.10.005. [DOI] [PubMed] [Google Scholar]
  58. Bhattacharjee S. DLS and zeta potential-what they are and what they are not? J. Controlled Release. 2016;235:337–351. doi: 10.1016/j.jconrel.2016.06.017. [DOI] [PubMed] [Google Scholar]
  59. Li W. L. Lai H. Sun C. H. Lin Y. Y. Sun Y. H. Nan J. M. Heterojunction of SnO2/Sn nanoparticles coated by graphene-like porous carbon as ultrahigh capacity anode of lithium-ion batteries. J. Alloys Compd. 2023;948:169811. doi: 10.1016/j.jallcom.2023.169811. [DOI] [Google Scholar]
  60. Zhang Y. Zhou J. Feng Q. Chen X. Hu Z. Visible light photocatalytic degradation of MB using UiO-66/g-C3N4 heterojunction nanocatalyst. Chemosphere. 2018;212:523–532. doi: 10.1016/j.chemosphere.2018.08.117. [DOI] [PubMed] [Google Scholar]
  61. Kareem M. A. Bello I. T. Shittu H. A. Sivaprakash P. Adedokun O. Arumugam S. Synthesis, characterization, and photocatalytic application of silver doped zinc oxide nanoparticles. Cleaner Mater. 2022;3:100041. doi: 10.1016/j.clema.2022.100041. [DOI] [Google Scholar]
  62. Lachheb H. Puzenat E. Houas A. Ksibi M. Elaloui E. Guillard C. Herrmann J. M. Photocatalytic degradation of various types of dyes (Alizarin S, Crocein Orange G, Methyl Red, Congo Red, Methylene Blue) in water by UV-irradiated titania. Appl. Catal., B. 2002;39(1):75–90. doi: 10.1016/S0926-3373(02)00078-4. [DOI] [Google Scholar]
  63. He R. Zhou J. Fu H. Zhang S. Jiang C. Room-temperature in situ fabrication of Bi2O3/g-C3N4 direct Z-scheme photocatalyst with enhanced photocatalytic activity. Appl. Surf. Sci. 2018;430:273–282. doi: 10.1016/j.apsusc.2017.07.191. [DOI] [Google Scholar]
  64. Iben Ayad A. Luart D. Ould Dris A. Guénin E. Kinetic analysis of 4-nitrophenol reduction by “water-soluble” palladium nanoparticles. Nanomaterials. 2020;10(6):1169. doi: 10.3390/nano10061169. [DOI] [PMC free article] [PubMed] [Google Scholar]
  65. Liu Y. Feng P. Wang Z. Jiao X. Akhtar F. Novel fabrication and enhanced photocatalytic MB degradation of hierarchical porous monoliths of MoO3 nanoplates. Sci. Rep. 2017;7(1):1845. doi: 10.1038/s41598-017-02025-3. [DOI] [PMC free article] [PubMed] [Google Scholar]
  66. Li X. Pi Y. Wu L. Xia Q. Wu J. Li Z. Xiao J. Facilitation of the visible light-induced Fenton-like excitation of H2O2via heterojunction of g-C3N4/NH2-Iron terephthalate metal–organic framework for MB degradation. Appl. Catal., B. 2017;202:653–663. doi: 10.1016/j.apcatb.2016.09.073. [DOI] [Google Scholar]
  67. Zhang S. Liu Y. Gu P. Ma R. Wen T. Zhao G. Li L. Ai Y. Hu C. Wang X. Enhanced photodegradation of toxic organic pollutants using dual-oxygen-doped porous g-C3N4: mechanism exploration from both experimental and DFT studies. Appl. Catal., B. 2019;248:1–10. doi: 10.1016/j.apcatb.2019.02.008. [DOI] [Google Scholar]
  68. Geldasa F. T. Kebede M. A. Shura M. W. Hone F. G. Experimental and computational study of metal oxide nanoparticles for the photocatalytic degradation of organic pollutants: a review. RSC Adv. 2023;13(27):18404–18442. doi: 10.1039/D3RA01505J. [DOI] [PMC free article] [PubMed] [Google Scholar]
  69. Jari Y. Favier L. Necibi M. C. Gourich B. Vial C. Imgharn A. Najid N. Barhoumi A. Chafi M. Alonzo V. Roche N. Enhanced visible-light degradation and mineralization of Bisphenol A using Cu-doped TiO2 photocatalysts: characterization, effectiveness, mechanism and DFT insights. Water Resour. Ind. 2026;35:100335. doi: 10.1016/j.wri.2025.100335. [DOI] [Google Scholar]
  70. Ahmed T. Y. Aziz S. B. Dannoun E. M. New photocatalytic materials based on alumina with reduced band gap: a DFT approach to study the band structure and optical properties. Heliyon. 2024;10(5):e27029. doi: 10.1016/j.heliyon.2024.e27029. [DOI] [PMC free article] [PubMed] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

RA-OLF-D6RA07029A-s001

Data Availability Statement

The datasets generated and/or analysed during the current study are available in the manuscript. Additional data or computational details can be made available by the corresponding author upon reasonable request.

Supplementary information (SI): the Cartesian coordinates for graphene, graphene oxide (GO), reduced graphene oxide (rGO), SnFe2O4, and the SnFe2O4–rGO composites (1 and 2). See DOI: https://doi.org/10.1039/d6ra07029a.


Articles from RSC Advances are provided here courtesy of Royal Society of Chemistry

RESOURCES