Skip to main content
. Author manuscript; available in PMC: 2012 Apr 5.
Published in final edited form as: Langmuir. 2011 Mar 14;27(7):4142–4148. doi: 10.1021/la200114s

Table 1.

Synthesis conditions used and the resultant microgel properties

Code Initiator
Concentration
(mM)
Initiator Synthesis
Temperature
(°C)
Rh at 22
°C
(nm)
Microgel
Yield
ζ-potential
(mV)
22 °C 40
°C
45A1 1 APS 45 - 13% - -
70A1 1 APS 70 336 79% −15.4 −33.0
37AT1 1 APS+TEMED 37 771 35% −2.36 −29.7
45AT1 1 APS+TEMED 45 358 72% −9.16 −28.2
45AT0.5 0.5 APS+TEMED 45 366 51% −2.46 −23.9
45AT2 2 APS+TEMED 45 358 60% −7.76 −32.8
55AT1 1 APS+TEMED 55 317 70% −7.18 −32.2
70AT1 1 APS+TEMED 70 278 60% −6.29 −36.1
45V 1 V50 45 - 18% - -
37VL 1 V50+UV 37 597 63% 8.65 23.5
45VL 1 V50+UV 45 436 78% 11.2 32.2