Abstract
Environmentally Degradable Parameter (Ed K) is of importance in the describing of biodegradability of environmentally biodegradable polymers (BDPs). In this study, a concept Ed K was introduced. A test procedure of using the ISO 14852 method and detecting the evolved carbon dioxide as an analytical parameter was developed, and the calculated Ed K was used as an indicator for the ultimate biodegradability of materials. Starch and polyethylene used as reference materials were defined as the Ed K values of 100 and 0, respectively. Natural soil samples were inoculated into bioreactors, followed by determining the rates of biodegradation of the reference materials and 15 commercial BDPs over a 2-week test period. Finally, a formula was deduced to calculate the value of Ed K for each material. The Ed K values of the tested materials have a positive correlation to their biodegradation rates in the simulated soil environment, and they indicated the relative biodegradation rate of each material among all the tested materials. Therefore, the Ed K was shown to be a reliable indicator for quantitatively evaluating the potential biodegradability of BDPs in the natural environment.
Introduction
Plastic has many applications in our daily life such as food packaging. Over the last 20 years, the production and consumption of polymeric materials have made plastic pollution a significant environmental issue [1]. It has been estimated that 2% of all plastics eventually reach the environment, thus contributing considerably to a currently acute ecological problem [2]. In addition to causing pollution, the manufacture of plastics consumes oil. As oil resources become increasingly scarce world wide, predictions have estimated that oil reserves are available up to 2040 [3]. Hence, possible oil shortages and plastic pollution have driven the development of biobased and biodegradable polymers (BBDPs) derived from renewable resources [4]. Environmentally biodegradable polymers (BDPs) are kinds of environmentally-friendly materials, which can be degraded into carbon dioxide and water by microorganisms in natural environment. BDPs are sustainable materials with low environmental impacts, low energy consumption and high biodegradability compared to oil-based materials [5].
BDPs can be divided into two classes according to the source they based. One class is non-biobased BDPs such as polyethylene glycol (PEG), polyethylene oxide (PEO) [6], polyester amide (PEA) [7], poly (propylene carbonate) (PPC) [8] and polycaprolactone (PCL) [9]. The other class is biobased BDPs which can be divided into three kinds: microbial polymers such as pullulan, curdlan, polyhydroxyalkanoates (PHA) [10], [11]; chemically synthesized polymers such as poly (butylene succinate) (PBS) [12] and polylactic acid (PLA) [13]; natural polymers such as chitosan, cellulose and polysaccharide [14]–[16].
Just as the petroleum based polymers polyethylene (PE) and polypropylene (PP), BDPs have parameters characterizing their physical and chemical properties, such as melting temperature (T m), glass transition temperature (T g), Young's modulus (E), solubility parameter (δ), etc [17]. However, a single parameter describing environmental degradability of BDPs has not yet been defined. Biodegradability has always been considered as an important character for BDPs, but until recently a single environmental degradability parameter (Ed K) has not yet been defined.
Methods for measuring biodegradability can be divided into two principal groups: (i) direct measurement of parent BDPs concentrations; (ii) indirect measurement of parent BDPs bioconversion, such as carbon dioxide production [18]–[21]. For practical and legislative purposes, a number of biodegradation test procedures have been standardized to determine the biodegradability of materials. These methods include, among others, ISO 14851, ISO 14852, ISO 14855, ISO 846, ASTM D 5209-91, ASTM D 5247-92, etc. Currently, when a new BDP is synthesized, outdoor and indoor methods are used to evaluate the degradability of the material. These standard methods can perfectly determine whether a certain material is a BDP under certain experimental condition, and give the biodegradation rate of BDPs, but can not manifest their advantages and disadvantages in the aspect of degradability compared with other BDPs. The aim of the present work is to define the environmentally degradable parameter, Ed K, and describe the methods for Ed K determination.
Materials and Methods
Ethics Statement
We state that “No specific permits were required for the described field studies.” We state that “No any relevant permissions/permits required for our observational or field studies.” For any locations/activities for which specific permission was not required, we state that a. no specific permissions were required for these locations/activities; b. that the location is not privately-owned or protected in any way and c. that the field studies did not involve endangered or protected species.
BDPs selected
Fifteen BDPs were selected as the only carbon and energy sources in a mineral salt solution, their names, molecular weights and makers are summarized in Table 1.
Table 1. BDPs and reference materials.
Material | M w | Supplier |
Pullulan | M w 200,000 | Tokyo Kasei Kogyo Co. Ltd., Japan |
Curdlan | M w 40,000–600,000 | Wako Pure Chemical Industries, Ltd., Japan |
Chitosan | M w 120,000–300,000 | Shanghai Boao Co. Ltd., China |
Cellulose | M w 5,000–250,000 | Merck Co. Ltd., Germany |
Poly (3-hydroxybutyrate-co- 3-hydroxyvalerate), PHBV | M n 750,000 | ZENEKA Co. Ltd., Japan |
Poly (3-hydroxybutyrate-co- 3-hydroxyhexanoate), PHBHHx | M n 160,000 | KANEKA Co. Ltd., Japan |
Poly (ε-caprolactone), PCL | M n 50,000 | SHOWA Co. Ltd., Japan |
Poly (butylenes succinate), PBS | M n 140,000 | SHYUWA Polymer Co. Ltd., Japan |
Poly (butylenes succinate-co- adipate), PBSA | M n 140,000 | SHYUWA Polymer Co. Ltd., Japan |
Poly (vinyl alcohol), PVA | Mn 1,750 | Shanghai Reagent Corporation, Chinese Medicine Corporation |
Poly (ethylene glycol), PEG | M n 2,000 | Shanghai Reagent Corporation, Chinese Medicine Corporation |
Poly (ethylene oxide), PEO | M n 100,000 | Liansheng Chemical Engineering Ltd. Co., Shanghai, China |
Poly (propylene carbonate), PPC | M n 200,000 | Mengxi High Technol Co. Ltd., China |
Poly (lactic acid), PLA | M n 200,000 | SHIMADZU Co. Ltd., Japan |
Poly (ester amide), PEA | M n 200,000 | Chengdu Institute of Organic-chemistry, Chinese Academy of Science |
Soluble starch | M w 300,000– 3,000,000 | Wako Pure Chemical Industries, Ltd., Japan |
Polyethylene, PE | M w 200,000 | Daqing petrochemicals Co. Ltd., Daqing, Heilongjiang Province, China |
Mineral salt solution preparation
ISO14852 method was used to detect the degradability of the above materials, in which two different concentration mineral salt solutions were given. The low one was used to represent the natural environment while the high one could accelerate the microorganism reproduction in the inoculation solution. A mineral salt concentration between the low and high concentrations was used here to simulate the natural environment and to shorten the detection time. The mineral salt solution contained 100 mL/L solution A, 10 ml/L solution B, 1 ml/L solution C and 1 ml/L solutionD and adjusted to pH 7.4. Solution A consisted of (g/L): 8.5 KH2PO4, 21.75 K2HPO4, 33.4 Na2HPO4•12 H2O and 0.5 NH4Cl. Solution B, C and D contained 22.5 g/L MgSO4•7 H2O, 36.4 g/L CaCl2•2 H2O and 0.25 g/L FeCl3•6 H2O respectively. Preliminary results indicated that this mineral salt solution composition was suitable for the growth of microorganisms and the secretion of degrading enzymes.
Materials mass determination
Because ISO14852 method required that the total organic carbon (TOC) content of the test material in the bioreactor was in the range of 100–2000 mg/L, and that the C/N mass ratio should be controlled at 40∶1, the TOC was determined to be 520 mg/L according to the TON (13 mg/L) in mineral salt solution. 400 mg starch in 300 mL mineral salt solution yielded a TOC of 518 mg/L, which was conveniently close to the recommendation of 520 mg/L. This TOC was used as the basis of all further tests and weights of the other polymers were calculated accordingly. The total organic carbon content of the test materials determined as the equation below:
The TOC values of PHBHHx, PHBV, PBSA and PEA were correlated with the monomer content and were provided by the suppliers. The masses for each material added into the bioreactors are shown in Table 2.
Table 2. Xc of materials and the mass added into bioreactor.
Materials | Xc (%) a | m material (mg) b |
Starch | 38.9 | 400.0 |
Pullulan | 44.4 | 350.0 |
Curdlan | 36.3 | 428.0 |
PHBHHx | 60.0 | 259.0 |
PHBV | 58.1 | 268.0 |
PEA | 64.3 | 242.0 |
PCL | 63.2 | 246.0 |
Cellulose | 56.3 | 276.0 |
Chitosan | 40.4 | 384.0 |
PEG | 54.6 | 285.0 |
PVA | 54.6 | 285.0 |
PEO | 54.6 | 285.0 |
PPC | 47.1 | 330.0 |
PBSA | 57.8 | 269.0 |
PBS | 56.8 | 274.0 |
PLA | 49.5 | 314.0 |
PE | 85.7 | 181.0 |
a: Xc: Total organic carbon of each BDPs, expressed in percent. The values of the TOC for each BDP were constant as they were counted from their chemical formulation.
b: m material (mg) : the mass of each BDPs added into the flask, it was calculated by (518 mg/L× 0.3 L)/Xc.
Preparation of inoculation solution
Activated sludge, compost or fertile soil could be used as inoculum mentioned in the standard method. Here, the farmland soil used as inoculum was from Zhouli village, Xiqing district of Tianjin City (collected at a depth of 0–10 cm). The soil used to inoculate the bioreactor was analyzed according to the standard methods [22], and its properties were as follows: pH (H2O) 8.20, pH (KCl) 7.90, 17.86% H2O, 2.18% C, 2.23% H and 0.85% N. The total number of microorganisms (including bacteria and fungi) in the soil was 6.9×107 per gram of wet soil using direct plate counting method which consisted of evenly spreading the diluted sample over an LB agar plate under aerobic condition at 30°C for 48 hours. LB agar medium contained yeast extract 5 g/L, tryptone 10 g/L, NaCl 10 g/L and agar 15 g/L. Using this method yielded colonies that form on the surface of the agar. The inoculation solution was prepared by adding 100 g soil to 1000 ml sterile mineral salt solution, stirring for 30 min at 4°C. After allowing the solution to stand for 30 min, the upper suspension was made as the inoculum.
Reference material selection
Carbon dioxide from the BDPs was detected and the biodegradation rate was calculated from the ratio of released CO2 to the theoretical amount of CO2. The apparatus used to detect the release of CO2 by BDP degradation is shown in Figure 1. PE and starch were used as reference materials, because PE was not degraded over 32 years [23] and starch could be degraded most easily [24]. We defined the Ed K value of PE as 0, and the Ed K value of starch as 100. Therefore, the Ed K of other BDPs should lie between 0 and 100.
Determination of testing time required for Ed K determination
To determine the time for Ed K detection, the time for starch complete degradation was measured in preliminary experiments. Results indicated that 400 mg starch could be completely degraded in 14 days in 300 ml mineral salt solution. Therefore, the detection time used for determining the Ed K of other BDPs was fixed at 14 days.
Degradation Method
The degradation experiments were carried out using the device shown in Figure 1. Atmospheric air (78% N2, 21% O2 and 0.03% CO2) was supplied by an air pump at 50–100 mL/min. Flasks b and c were filled with 300 ml NaOH solution (10 M) to remove CO2 from pumped air. Flask d was filled with 200 ml Ba(OH)2 solution (0.0125 M) to indicate complete removal of CO2 in pumped air. Flask e was the bioreactor filled with 300 ml mineral salt solution. A thermostatic magnetic stirrer was employed to control the temperature and rotation speed in the bioreactor. Flask f and g were filled with 250 ml NaOH solution (0.05 M) to absorb the CO2 released in the bioreactor during biodegradation process. Flask h was filled with 200 ml Ba(OH)2 solution (0.0125 M) to indicate complete removal of CO2 released from the bioreactor. Beaker i was filled with water and used to confirm the airtightness of the devices. Various masses of BDPs calculated to give a TOC of 518 mg/L were added. into the bioreactor containing 300 ml mineral salt solution and 24.0 ml inoculation solution was added also. The mixture reacted for 14 days at 30°C. A blank control and reference materials were also prepared. CO2 released was absorbed by NaOH and the consumption of NaOH was determined by titration. All measurements of titration were repeated three times. In the CO2 absorption process, NaOH is present in excess and the chemical reaction is:
2NaOH+CO2 = Na2CO3+H2O (a).
Then, flasks f and g were pooled together and 10 ml of the NaOH solution was sampled and titrated using 0.05 M HCl. The chemical reaction equations are:
NaOH+HCl = NaCl+H2O (b);
Na2CO3+HCl = NaCl+NaHCO3 (c).
Phenolphthalein was used as indicator. Phenolphthalein will turn to colorless from red when the pH of the solution become into neutral. At this point, colligating equation (a), (b) and (c), when CO2 is in excess, the reaction is:
NaOH+CO2 = NaHCO3 (d).
ΔV of NaOH equals 10 ml of NaOH minus the volume of titration HCl used.
Results
Introduction of equations
The only carbon source and energy resource in the mineral salt solution were the BDPs being tested. The inoculum was fertile soil suspension. A device capable of detecting CO2 release from BDPs during degradation was designed in accordance with ISO14852 (Figure 1). The consumption of NaOH was calculated, from which the amount of released CO2 was calculated as in equation (1):
(1) |
where ∑(CO2) is the amount of CO2 released by the material, ΔV is volume of NaOH solution consumed (ml), 10 is the sample volume of NaOH (ml), 250 is the total volume of NaOH solution in the absorption bottle (ml) (bottle f and g in Figure 1), 0.05 is the concentration of NaOH solution (M), and 44 g/mol is the molecular weight of CO2.
The biodegradation rate or potential biodegradability of BDPs in the natural environment was calculated from the ratio of the amount of CO2 released to the maximum theoretical amount of CO2 that could be released, as in equation (2):
(2) |
where BioMaterial is the biodegradation rate of the test material, Σ(CO2)Material is the total amount of CO2 released by the material, Σ(CO2)Blank is the amount of CO2 released in the blank bottle and ThCO2 is the maximum theoretical amount of CO2 that could be released.
ThCO2 is calculated as in equation (3):
(3) |
where m is the mass of the material to be determined (g), Xc is the organic carbon content of the material to be determined, and 44 g/mol and 12 g/mol are the molecular weight of CO2 and atomic weight of carbon respectively. Since TOC was fixed at 518 mg/L and nutrient salt volume was 300 mL for all polymers, ThCO2 was 569.8 mg in all cases.
Calculation of Ed K
The biodegradation rate of BDPs could be calculated according the following method, the environmentally degradable parameter (Ed K) was calculated as in equation (4):
(4) |
where Ed K Materials is the environmental degradability parameter of the test material, BioStarch is the biodegradation rate of starch, BioMaterial is the biodegradation rate of the test material, and BioPE is the biodegradation rate of PE.
Combining equations (2) and (4), the environmental degradability parameter is calculated as in equation (5):
(5) |
Because the TOC content of PE, starch and the test materials were identical, so their theoretical amounts of CO2 were the same. Meanwhile, the amount of CO2 released by PE was equal to that of the blank control where the only carbon source was derived from the inoculation solution. Hence, PE was not degraded at all in the inoculated mineral salt solution. Therefore, equation (5) can be simplified as in equation (6):
(6) |
Combining equations (1) and (6) yields equation (7), the EdK value of test materials can be calculated by measuring the consumption of NaOH solution by CO2 released during degradation of the material:
(7) |
where Δ VMaterial is the volume of NaOH solution consumed by CO2 released during the degradation of test material, ΔVStarch is the volume of NaOH solution consumed by CO2 released during the degradation of starch, and ΔVPE is the volume of NaOH solution consumed by CO2 released during the degradation of PE.
Fifteen different BDPs were detected by this method, and ThCO2, CO2 released, biodegradation rate and Ed K were listed in Table 3.
Table 3. Biodegradation rate and Ed K of BDPs.
Materials | ThCO2 (mg)a | EvCO2 (mg)b | Biodegradation rate (%)c | EdK d |
starch | 569.8 | 446.40±9.92 | 78.34±1.74 | 100.00±0.00 |
pullulan | 569.8 | 420.37±7.70 | 73.77±1.35 | 94.22±3.74 |
curdlan | 569.8 | 368.12±10.19 | 64.60±1.79 | 82.50±3.13 |
PHBHHx | 569.8 | 354.20±5.04 | 62.16±0.88 | 79.36±1.28 |
PHBV | 569.8 | 304.70±3.81 | 53.47±0.67 | 68.29±2.28 |
PEA | 569.8 | 206.80±10.49 | 36.29±1.84 | 46.34±2.58 |
PCL | 569.8 | 146.30±3.97 | 25.68±0.7 | 32.77±0.21 |
cellulose | 569.8 | 142.45±3.43 | 25.00±0.6 | 31.93±1.36 |
chitosan | 569.8 | 84.70±2.40 | 14.86±0.42 | 18.98±0.71 |
PEG | 569.8 | 68.20±2.20 | 11.97±0.39 | 15.28±0.42 |
PVA | 569.8 | 28.60±2.52 | 5.02±0.44 | 6.41±0.53 |
PEO | 569.8 | 21.45±1.46 | 3.76±0.26 | 4.81±0.43 |
PPC | 569.8 | 19.25±1.46 | 3.38±0.26 | 4.31±0.27 |
PBSA | 569.8 | 16.50±1.46 | 2.90±0.26 | 3.70±0.32 |
PBS | 569.8 | 11.00±0.55 | 1.93±0.10 | 2.47±0.16 |
PLA | 569.8 | 5.50±1.46 | 0.97±0.26 | 1.23±0.32 |
PE | 569.8 | 0.00±0.00 | 0.00±0.00 | 0.00±0.00 |
a: ThCO2: the theoretically released CO2 of each material; b: EvCO2: The average with standard deviation of three independent titration results for the actually released CO2 of material to be determined in the degradation process; c: Biodegradation rate: the value of biodegradation rate calculated via formula 2; d: Ed K: the degradable parameter calculated via formula 7.
Discussion
In our, pre-exprement we observed that the amount of CO2 released by PE was equal to that of the blank control where the only carbon source was derived from the inoculation solution. PE was not degraded at all in the inoculated mineral salt solution. From the calculation of Ed K, we can see that the values of blank control will be removed as it is a common factor. From equation (7), we only need to know the ΔV of material, PE and starch to calculate Ed K.
Among 15 BDPs tested, the ranking of some BDPs according to the Ed K values was consistent with some of the conclusions in the aspect of biodegradability reported in the literatures although the methods used were different. Rosa et al. reported that PHBV was the most biodegradable and PCL the least, when PHB, PHBV and PCL were buried in soil compost at pH 11.0 [2]. In our study, the Ed K values of PHBV and PCL were 68.29±2.28 and 32.77±0.21 respectively (Table 3). It indicated that the biodegradability of PHBV used in the study was better than that of PCL, which was in accordance with Rosa et al.'s conclusion although PHBV used may be different in monomer composition. It was interesting that the soil sample used in this study and Rosa et al.'s study were different. Therefore, investigation of the relationship between the microbial composition and the degradation of BDPs needs to be done in the future studies. According to Song et al.'s study, PLA belonged to the slow biodegradation rate plastic with mass loss<5% after 90 days [25]. This was also in accordance our observation that PLA had a biodegradation rate of 0.97±0.26 % with the Ed K value of 1.23±0.32 (Table 3).
Fifteen BDPs were detected by this method, and ThCO2, CO2 released, biodegradation rate and Ed K were listed in Table 3. As expected, Ed K of natural polymers was higher than synthetic polymers. Higher Ed K values indicate faster biodegradation rate of the material in the natural environment. The Ed K of PLA was only 1.2, which was consistent with our previous studies that indicated that PLA was not significantly degraded when buried in soil for 3 years [26]. As indicated in ISO14852, employing microorganisms from different sources yields different degradation results. If the detection system could be unified by using a defined inoculum, for example a mixed solution of pure microorganism with prescribed concentrations, just as Guo et al. [27] described, then the same Ed K of BDPs could be obtained in any laboratory of the whole world.
In this study, a concept of Environmentally Degradable Parameter (Ed K) was introduced. A formula was deduced to calculate the value of Ed K for 15 commercial BDPs. The Ed K was shown to be a reliable indicator for quantitatively evaluating the potential biodegradability of BDPs in the nature environment.
Acknowledgments
We wish to thank Prof. Takeuchi Shugeya in Toyama University, Japan for his providing some samples of BDPs. Additionally, we would like to express our thanks to Prof. Choichiro Shimasaki, Masami Inoue and associated Prof. Shin Ono in Toyama University, Japan for their valuable discussions. Also, we would like to express our thinks to Prof. Ramani Narayan in Michigan State University, USA and Dr. Yunxuan Weng in Degradable Plastics Committee, Plastics Processing Industry Association, China for their valuable advice.
Footnotes
Competing Interests: The authors have declared that no competing interests exist.
Funding: The authors gratefully acknowledge the financial support from National Key Basic Research Program of China ("973" Program) 2012CB725204, National High Technology Research and Development Program of China ("863" Program) 2012AA021505, Natural Science Foundation of China grant nos. 31070039, 51073081 and 51073081, Project of Tianjin, China 1JCYBJC09500. The funders had no role in study design, data collection and analysis, decision to publish, or preparation of the manuscript.
References
- 1.Gross RA, Kalra B. Biodegradable polymers for the environment. Science. 2002;297:803–807. doi: 10.1126/science.297.5582.803. [DOI] [PubMed] [Google Scholar]
- 2.Rosa DS, Calil MR, Guedes CGF, Rodrigues TC. Biodegradability of Thermally Aged PHB, PHB-V, and PCL in Soil Compostage. J Polym Environ. 2004;12:239–245. [Google Scholar]
- 3.Shafiee S, Topal E. When will fossil fuel reserves be diminished? Energ Policy. 2009;37:181–189. [Google Scholar]
- 4.Montgomery R. Development of biobased products. Bioresour Technol. 2004;91:1–29. doi: 10.1016/s0960-8524(03)00154-8. [DOI] [PubMed] [Google Scholar]
- 5.Song JH, Murphy RJ, Narayan R, Davies GBH. Biodegradable and compostable alternatives to conventional plastics. Phil Trans R Soc B. 2009;364:2127–2139. doi: 10.1098/rstb.2008.0289. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 6.Li J, Li X, Ni XP, Wang X, Li HZ, et al. Self-assembled supramolecular hydrogels formed by biodegradable PEO–PHB–PEO triblock copolymers and α-cyclodextrin for controlled drug delivery. Biomaterials. 2006;27:4132–4140. doi: 10.1016/j.biomaterials.2006.03.025. [DOI] [PubMed] [Google Scholar]
- 7.Ai YP, Shi ZL, Guo WX. A new type of unsaturated poly (ester-amide): Synthesis and compressive strength. Mate Des. 2009;30:892–895. [Google Scholar]
- 8.Goel R, Zaidi MGH, Soni R, Lata K, Shouche YS. Implication of Arthrobacter and Enterobacter species for polycarbonate degradation. Int Biodeter Biodegr. 2008;61:167–172. [Google Scholar]
- 9.Zhao Q, Tao J, Yam RCM, Mok ACK, Li RKY, et al. Biodegradation behavior of polycaprolactone/rice husk ecocomposites in simulated soil medium. Polym Degrad Stabil. 2008;93:1571–1576. [Google Scholar]
- 10.Verlinden RAJ, Hill DJ, Kenward MA, Williams CD, Radecka I. Bacterial synthesis of biodegradable polyhydroxyalkanoates. J Appl Microbiol. 2007;102:1437–1449. doi: 10.1111/j.1365-2672.2007.03335.x. [DOI] [PubMed] [Google Scholar]
- 11.Doi Y. Unnatural biopolymers. Nat Mater. 2002;1:207–208. doi: 10.1038/nmat783. [DOI] [PubMed] [Google Scholar]
- 12.Nikolic MS, Djonlagic J. Synthesis and characterization of biodegradable poly (butylene succinate-co-butylene adipate)s. Polym Degrad Stabil. 2001;74:263–270. [Google Scholar]
- 13.Tokiwa Y, Jarerat A. Biodegradation of poly (L-lactide). Biotechnol Lett. 2004;26:771–777. doi: 10.1023/b:bile.0000025927.31028.e3. [DOI] [PubMed] [Google Scholar]
- 14.Filho GR, Monteiro DS, Meireles CS, Assunção RMN, Cerqueira DA, et al. Synthesis and characterization of cellulose acetate produced from recycled newspaper. Carbohydr Polym. 2008;73:74–82. [Google Scholar]
- 15.Mourya VK, Inamdar NN. Chitosan-modifications and applications: Opportunities galore. React Funct Polym. 2008;68:1013–1051. [Google Scholar]
- 16.Ding Q, LaBelle M, Yang BY, Montgomery R. Physicochemical studies of extracellular polysaccharides of Erwinia chrysanthemi spp. Carbohydr Biopolym. 2003;51:333–346. [Google Scholar]
- 17.Rubinstein M, Colby RH. New York: Oxford University Press; 2003. Polymer Physics.454 [Google Scholar]
- 18.ISO 14852: Determination of the ultimate aerobic biodegradability of plastic materials in an aqueous medium – Method by analysis of evolved carbon dioxide. 1999.
- 19.ISO 14855: Determination of the ultimate aerobic biodegradability and disintegration of plastic materials under controlled composting conditions – Method by analysis of evolved carbon dioxide. 1999.
- 20.ISO 14851: Determination of the ultimate aerobic biodegradability of plastic materials in an aqueous medium – Method by measuring the oxygen demand in a closed respirometer. 1999.
- 21.ISO 846: Evaluation of the potential biodegradability and disintegration of plastic materials by the action of the specific microorganisms. 1997.
- 22.Ishikuri S. Japan: YOKENDO Press; 1992. New compilation soil microbiology experimental method.406 [Google Scholar]
- 23.Otake Y, Kobayashi T, Asabe H, Murakami N, Ono K. Biodegradation of low-density polyethylene, polystyrene, polyvinyl chloride, and urea formaldehyde resin buried under soil for over 32 years. J Appl Polym Sci. 1995;56:1789–1796. [Google Scholar]
- 24.Ryan SM, Fitzgerald GF, Sinderen D. Screening for and identification of starch-, amylopectin- and pullulan-degrading activities in bifidobacterial strains. Appl Environ Microbiol. 2006;72:5289–5296. doi: 10.1128/AEM.00257-06. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 25.Song JH, Murphy RJ, Narayan R, Davies GBH. Biodegradable and compostable alternatives to conventional plastics. Phil Trans R Soc B. 2009;364:2127–2139. doi: 10.1098/rstb.2008.0289. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 26.Mizuno W, Sano M, Song CJ, Nakatani T, Yoshida M, et al. Evaluation of biodegradability of several biodegradable plastics in natural environments. KOBUNSHI RUNBUNSHU. 2003;60:622–628. [Google Scholar]
- 27.Guo WB, Tao J, Yang C, Zhao Q, Song CJ, et al. The rapid evaluation of material biodegradability using an improved ISO 14852 method with a microbial community. Polym Test. 2010;29:832–839. [Google Scholar]