Abstract
Iso-selective initiators for the ring-opening polymerization (ROP) of rac-lactide are rare outside of Group 13. We describe the first examples of highly iso-selective lutetium initiators. The phosphasalen lutetium ethoxide complex shows excellent iso-selectivity, with a Pi value of 0.81–0.84 at 298 K, excellent rates, and high degrees of polymerization control. Conversely, the corresponding La derivative exhibits moderate heteroselectivity (Ps=0.74, 298 K). Thus, the choice of metal center is shown to be crucial in determining the level and mode of stereocontrol. The relative order of rates for the series of complexes is inversely related to metallic covalent radius: that is, La>Y>Lu.
Keywords: iso-selectivity, lactide, lanthanum, lutetium, ring-opening polymerization
Polylactide (PLA), a degradable polymer obtained from renewable resources, is one of the leading commercial alternatives to petrochemical plastics.[1] PLA is produced by the metal-catalyzed ring-opening polymerization (ROP) of lactide (LA).[2] The central challenge in this field of catalysis is to combine high rates with excellent stereocontrol, ideally without the need for expensive chiral auxiliaries or ligands.[3] Iso-selectivity using rac-LA is especially important and useful because the product, stereoblock/complex PLA, has superior properties.[4] For example, it is a crystalline polymer with a higher melting temperature (Tm) and better mechanical properties than isotactic poly-L-lactide (PLLA). In some cases, Tm is elevated by as much as 50 °C, greatly improving thermal stability and enabling PLA to compete as an engineering polymer.[5] However, rac-LA iso-selective catalysts remain scarce, with the majority being chiral aluminum salen complexes or derivatives.[3b, 4a], [6] Although these compounds show impressive degrees of stereocontrol, they are often extremely slow and require unacceptably high catalyst loadings, typically taking hours or days to reach completion even at 1 mol % catalyst loading. There are only a handful of other, non-aluminum based, iso-selective catalysts,[7] the structures of three of the most selective of these are shown in Figure 1.[8] In 2008, Arnold and co-workers reported a homochiral yttrium complex that showed good iso-selectivity (C, Pi=0.75, 298 K).[8a,b] Subsequently, we reported yttrium phosphasalen complexes (Figure 1, structures A and B), which combined very high rates with promising iso-selectivity (Pi=0.74, 298 K).[8c]
Herein, we report the performance of lutetium and lanthanum phosphasalen complexes. For such Group 3 lanthanide complexes, the coordination geometries are predominantly influenced by steric factors. In this regard, it is relevant that lutetium has a slightly smaller covalent radius than yttrium (1.87 Å versus 1.90 Å), whilst lanthanum is significantly larger (2.07 Å).[9]
The use of different lanthanide centers enables an investigation of the influence of atomic size and coordination environment on polymer tacticity. Both metals have precedence in lactide ROP catalysis,[10] although lutetium is rarely investigated.[10b,e,f,h] Okuda and co-workers reported heteroselective (syndiotactic) dithiaalkanediyl-bridged bis(phenolato) yttrium and lutetium catalysts, but found that the stereocontrol decreased from Y to Lu.[10b,f] To our knowledge, there is no precedent for any iso-selective lutetium initiators.
The initiators were prepared in good overall yields, from the phosphasalen ligand, which was synthesized using an established procedure (Scheme 1).[8c] First, the ligand was deprotonated using potassium bis(trimethylsilyl)amide (5 equivalents), leading to quantitative conversion into the salt, as observed by the upfield shift (δP=23 ppm) of the signal for the phosphorus center in the 31P{1H} NMR spectrum. The lutetium phosphasalen chloride complex was formed, but not isolated, by reaction with LuCl3. One signal was observed for this species at δ=35 ppm in the 31P{1H} NMR spectrum. Addition of the relevant potassium alkoxide (ethoxide or tert-butoxide) led to the formation of the lutetium phosphasalen alkoxide complexes (1 and 2). A slight upfield shift was again observed for resonances in the 31P{1H} NMR spectra of both complexes (δP=34 ppm). Compounds 1 and 2 were isolated in good yields after recrystallization (55 % and 75 %, respectively).
The complexes were fully characterized by NMR spectroscopy and elemental analysis. At room temperature, the 1H NMR spectra of both 1 and 2 show broad resonance signals, indicative of fluxional processes, however, at 360 K coalescence occurs and clearly distinguishable signals are observed (see Figure S9 in the Supporting Information). At 298 K, the 31P{1H} NMR spectrum of compound 1 shows two signals in a 1:7 ratio, but on heating to 360 K a single sharp signal is observed at δ=34 ppm. The phosphasalen lanthanum tert-butyl alkoxide complex (3) was formed in an analogous fashion, albeit in a slightly lower yield (34 %). The intermediate chloride complex showed a single signal at δ=33 ppm in the 31P{1H} NMR spectrum. Addition of potassium tert-butoxide led to the formation of 3, which exhibited a single peak at lower chemical shift (δP=30 ppm). Crystals of all three new complexes suitable for single-crystal X-ray diffraction were isolated from solutions of the complexes in mixtures of cyclohexane and hexane (note that complex 3 crystallized with two independent molecules, 3 A and 3 B).
The structures of the complexes (Figure 2, Figures S1–S4) all show a severely distorted octahedral geometry at the metal center with trans angles in the ranges 144.52(14)–158.87(12)°, 141.9(3)–159.3(3)°, 127.11(16)–149.44(13)°, and 123.71(18)–146.96(13)° for 1, 2, 3 A, and 3 B, respectively. The yttrium analogue A [8c] has a similar geometry to those observed for 1 and 2. In each case, the pentacoordinate ligand occupies one hemisphere, leaving the alkoxide ligand isolated in the other hemisphere (Figure 2). The geometries of 1 and 2 are very similar, as would be expected with the only difference between the two complexes being a change in the alkoxide co-ligand. The lanthanum structure 3, however, shows marked differences. In addition to the expected elongation of all of the M=X bonds (Table S1) and the even greater distortion from ideal octahedral coordination angles at the metal center (see above), the O1⋅⋅⋅O21 phenoxide⋅⋅⋅phenoxide separation is markedly increased (3.074(4), 3.107(9), 3.154, 3.603(5), and 3.354(5) Å, measured for 1, 2, A (yttrium analogue),[8c] 3 A, and 3 B, respectively). Similarly, the “hole” in which the alkoxide ligand sits is larger in 3 A and 3 B than in either 1, 2, or yttrium analogue A.[8c] The closest approaches between the methyl group of the alkoxide and a carbon atom of the proximal phenyl ring are approximately 3.74, 3.83, 3.81, 4.67, and 4.13 Å for complexes 1, 2, A,[8c] 3 A, and 3 B, respectively. All four structures adopt asymmetric conformations that place one phenyl ring of one of the two PPh2 units—specifically a phenyl ring attached to P15—much closer to the alkoxide than the other three phenyl rings. There are noticeable differences in geometry between 3 A and 3 B, which are chemically identical, suggesting a distinct degree of flexibility in both the ligand and the coordination environment in 3. The most visually obvious difference is the orientation of the C48-containing phenyl ring bound to the P15 atom (the phosphorus closest to the alkoxide); in 3 A this ring is oriented approximately orthogonally to the N14=P15 bond, whereas in 3 B it is almost parallel to this bond (see Figures S3, S4).
Compounds 1–3 were tested as initiators for the ROP of rac-LA. Initially the experiments were conducted under standard conditions, using a 1 m solution of LA in THF at 298 K and with a 2 mm concentration of initiator. The progress of the polymerization was monitored by taking regular aliquots. All the new compounds (1–3) showed good to very good activities (Table 1). Based on the time required to achieve complete conversion of rac-LA into PLA, the order of activity decreased: La>Y>Lu. To quantify these observations, the polymerization kinetics were monitored (Figures S11, S12).
Table 1.
I | [I]:[iPrOH]:[LA] | t [h] | Conversion [%][d] | Mn,exp [g mol−1][e] | Mn,calcd [g mol−1] | PDI[e] | Pi[f] |
---|---|---|---|---|---|---|---|
1 | 1:500[g] | 8 | 81 | 101 700 | 58 300 | 1.06 | 0.80 |
1 | 1:1:500 | 9 | 84 | 38 900 | 60 500 | 1.07 | 0.75 |
1[ac] | 1:0.5:500 | 72 | 84 | 69 600 | 60 500 | 1.02 | 0.84 |
1[bc] | 1:0.5:200 | 48 | 90 | 36 000 | 26 000 | 1.02 | 0.83 |
2 | 1:500[g] | 8.25 | 86 | 53 400 | 61 900 | 1.02 | 0.82 |
2 | 1:350[g] | 5.5 | 86 | 38 300 | 43 300 | 1.09 | 0.82 |
2 | 1:250[g] | 3.5 | 86 | 34 900 | 31 000 | 1.02 | 0.84 |
2 | 1:200[g] | 2.75 | 89 | 27 800 | 25 600 | 1.05 | 0.81 |
2[ac] | 1:500[g] | 72 | 75 | 46 300 | 54 000 | 1.01 | 0.89 |
2[bc] | 1:200[g] | 48 | 81 | 22 800 | 23 300 | 1.02 | 0.89 |
3[a] | 1:1:500 | 20 s | 98 | 57 300 | 70 600 | 1.05 | 0.28 |
3 | 1:2:1000 | 20 s | 93 | 58 000 | 67 000 | 1.03 | 0.28 |
0.75 m [LA].
0.5 m [LA].
257 K.
Determined by integration of the methine region of the 1H NMR spectrum (LA, δ=4.98–5.08 ppm; PLA, δ=5.09–5.24 ppm).
Determined by GPC (gel permeation chromatography) in THF versus polystyrene standards (Mn values are corrected with a 0.58 factor).[11]
Determined by analysis of the homonuclear decoupled NMR spectrum according to the method first described by Coudane et al.[12]
No iPrOH added. I=initiator.
In all cases, a first-order dependence of the conversion rate on lactide concentration was observed, as evidenced by the linear fit of data to plots of ln([LA]t/[LA]0) versus time, from which the gradient corresponds to the kobs value. For 1 and 2, the kobs values are comparable at 6.3×10−5 s−1 and 7.5×10−5 s−1, respectively (Figure S11). This similarity is in line with expectations as the two compounds differ only in the nature of the alkoxide which is the initiating group. The two lutetium complexes 1 and 2 are approximately an order of magnitude slower than yttrium complexes A and B (kobs=6.9×10−4, 7.9×10−4 s−1). This finding is consistent with other examples of lutetium complexes.[10b,f,h,j], [13] In contrast, lanthanum complex 3 was an extremely fast initiator, enabling almost complete conversion of 1000 equivalents of LA [versus initiator, in the presence of isopropyl alcohol (2 equivalents)] in less than 20 seconds (Table 1). Such rates are beyond the limit of polymerization monitoring using aliquots and so no further kinetics studies were undertaken. Instead, the rate law for polymerization using 2 was investigated; kobs values were determined over a range of different initiator concentrations, ([2]=2–5 mm, at 298 K maintaining [LA]=1 m). In each case, the reactions were first-order in lactide concentration. The reactions also showed a first-order dependence on the concentration of initiator 2, as shown by the linear fit to the plot of kobs value versus the concentration of 2 (Figure 3). Thus, the overall rate law is second-order and the propagation rate constant, kp, is 5.08×10−5 m−1 s−1. As the rate depends on both initiator and lactide concentrations, the rate-limiting step could correspond to LA coordination or insertion, or a composite of both. Given that the order of rate (La>Y>Lu) is inversely related to the metal covalent radii and the expected Lewis acidities, it is hypothesized that the rate-limiting process is lactide insertion into the metal–alkoxide bond. Accordingly, the selection of the metal center controls the competing requirements for efficient polymerization, that is, the need for sufficient Lewis acidity to ensure rapid coordination, balanced with an alkoxide bond which is labile to substitution. The order of rates correlates with the metal–alkoxide bond lengths, as determined by single-crystal XRD experiments. The lanthanum–alkoxide bond is significantly longer than the lutetium–alkoxide and yttrium–alkoxide bonds (M–O21: 2.196(4), 2.060(3), 2.069(6) Å in 3 A (La), 1 (Lu), and A (Y), respectively).
Despite the high overall rates, the polymerizations remained very well controlled. In general, there was a close agreement between the theoretical and observed molecular weights, and the PLA had a narrow polydispersity index (PDI<1.10 in all cases, Table 1). Complexes 1 and 3 contain tert-butyl alkoxide as the co-ligand. This hindered alkoxide has been shown to undergo relatively slower initiation leading to Mn values exceeding those predicted.[8c] To overcome this limitation, isopropyl alcohol (0.5–1 equivalents) was added, which undergoes rapid and reversible exchange reactions leading to faster initiation and, in the case of 1, a very good match between the calculated and the experimental Mn values. In contrast, complex 2, containing an ethoxide co-ligand, enables very well-controlled polymerization without the need for any exogeneous alcohol.
Importantly, in addition to high rates and good polymerization control, the lutetium complexes 1 and 2 both polymerize rac-LA with a high iso-selective bias, as assessed by the Pi values which were determined by integration (normalized) of the homonuclear decoupled NMR spectra and comparison with the values predicted by Bernouillan statistics.[12] Compound 1 showed a significantly improved iso-selectivity compared to compound A (yttrium analogue) at 298 K (Pi=0.80 versus Pi=0.75). However, when one equivalent of isopropyl alcohol was added, the degree of iso-selectivity dropped (Pi=0.75 for 1, versus Pi=0.73 for compound A with iPrOH), presumably because of some scrambling of stereochemistry during chain transfer. Compound 2, which does not require any alcohol, was even more iso-selective at room temperature (Pi=0.82±0.02) and represents, to our knowledge, the highest iso-selectivity catalyst reported, excluding the aluminium salen complexes. As mentioned, although Pi values exceeding 0.95 are known for these chiral aluminum salen ligands, their activities are very low and the high loadings (more than 1 mol %) limit their applicability.
We next considered how to control the iso-selectivity. The Pi value remained high over a range of different catalyst loadings and therefore enabled the production of rather high Mn stereoblock PLA (Table 1). Stereocontrol is a kinetic phenomenon, therefore reducing the reaction temperature enables an increase in iso-selectivity, leading to a maximum Pi value of 0.89 at 257 K. Analysis of the defect tetrad signals in the homonuclear decoupled NMR spectrum indicate that iso-selectivity arises from a chain-end control mechanism (approximately a 1:1:1 ratio of sii:iis:isi; Figure S14). Differential scanning calorimetry (DSC) indicated the formation of semi-crystalline PLA with a Tm of 178 °C (Figure S16). The increased degree of iso-selectivity for complex 1 and 2 (versus yttrium analogues A and B) is tentatively proposed to be as a result of the smaller lutetium metal center enforcing a more sterically encumbered bonding geometry by the phosphasalen ligand.
Thus, we were surprised to discover that the lanthanum initiator, 3, exhibited moderate heteroselectivity (Ps=0.72). This is unexpected as a gradual decrease in stereocontrol on decreasing steric shielding is much more usual.[10c,d] We have previously observed that for a series of yttrium phosphasalen complexes, the stereocontrol switches from heterotactic (for tetracoordinate ligands) to isotactic (for pentacoordinate ligands).[8c] In contrast, the same pentacoordinate ligand bound herein to a series of lanthanide centers forms compounds with very closely related coordination geometries (see above), which leads to completely opposite stereoselectivities depending on the metal size. Insight into the propensity for an initiator to exhibit iso-selectivity or heteroselectivity can be gained by analysis of the NMR spectra. High-temperature 1H NMR experiments of the lutetium compounds show that signal coalescence is reached by 360 K (Figure S5, S6). Under the same conditions, resonance signals attributable to the lanthanum complex are still significantly broadened, indicating a more fluxional structure (Figure S7). 2D NMR spectroscopic experiments were even more informative. By using rotating-frame nuclear Overhauser effect spectroscopy (ROESY), it is possible to compare the fluxionalities of the complexes by monitoring proton-exchange events. It is important to note that all complexes showed proton exchange in the iminophosphorane bridges, in line with the broadened resonance signals in the 1H NMR spectra observed at 298 K. Lutetium complexes 1 and 2 showed limited further exchange, as did the yttrium analogues A and B.[8c] However, the lanthanum analogue 3 also showed significant exchange of the phenyl ring protons associated with the PPh2 groups (Figures S17, S18). These exchange events correspond to the protons experiencing the same magnetic environment on the NMR timescale, in this case they are indicative of rotations of the phenyl groups. Such rotations are consistent with 3 exhibiting a significantly more fluxional structure than 1 and 2. Interestingly, the rotations of the phenyl groups coordinated to the phosphorus are also manifested in the solid-state structures of the two independent molecules of compound 3: 3 A and 3 B (Figures S3, S4). Furthermore, previous studies using different yttrium derivatives, revealed that heteroselective catalysts exhibited free rotation of the phenyl groups whereas the iso-selective yttrium catalysts A and B showed no such fluxionality.[8c] Thus, these NMR studies add further weight to the hypothesis that iso-selectivity results from sterically congested metal complexes with limited fluxionality of the phosphorus substituents. In contrast, heteroselectivity is observed when using the larger metal center (La) which shows a more open coordination geometry and fluxionality of the phosphorus substituents.
In conclusion, we have reported highly iso-selective lutetium initiators. The phosphasalen lutetium ethoxide complex shows a Pi value of 0.82±0.02 at 298 K, moving to 0.89 at 257 K. In contrast, the analogous lanthanum initiator was heteroselective (Ps=0.72, 298 K). All initiators show excellent rates and high degrees of polymerization control. Both the relative order of rates and the mode and degree of stereocontrol for the series of complexes have been shown to be related to the metallic covalent radius. A larger metal center results in a higher observed rate (La>Y>Lu). The smaller metal center of lutetium promotes high iso-selectivity (higher than the previously reported yttrium), whilst the more open coordination geometry of lanthanum leads to moderate heteroselectivity. The type of stereocontrol appears to be associated with the level of rigidity imposed on the ligand. Thus, from a single ligand, two different modes of stereocontrol are possible: such switching is very unusual and warrants further investigation as an attractive route to control polymer properties.
Supporting information for this article is available on the WWW under http://dx.doi.org/10.1002/anie.201403643.
References
- [1a].Auras R, Harte B, Selke S. Macromol. Biosci. 2004;4:835–864. doi: 10.1002/mabi.200400043. [DOI] [PubMed] [Google Scholar]
- [1b].Ragauskas AJ, Williams CK, Davison BH, Britovsek G, Cairney J, Eckert CA, Frederick WJ, Hallett JP, Leak DJ, Liotta CL, Mielenz JR, Murphy R, Templer R, Tschaplinski T. Science. 2006;311:484–489. doi: 10.1126/science.1114736. [DOI] [PubMed] [Google Scholar]
- [1c].Williams CK, Hillmyer MA. Polym. Rev. 2008;48:1–10. [Google Scholar]
- [1d].Inkinen S, Hakkarainen M, Albertsson AC, Sodergard A. Biomacromolecules. 2011;12:523–532. doi: 10.1021/bm101302t. [DOI] [PubMed] [Google Scholar]
- [2a].O’Keefe BJ, Hillmyer MA, Tolman WB. J. Chem. Soc. Dalton Trans. 2001:2215. [Google Scholar]
- [2b].Dechy-Cabaret O, Martin-Vaca B, Bourissou D. Chem. Rev. 2004;104:6147. doi: 10.1021/cr040002s. [DOI] [PubMed] [Google Scholar]
- [2c].Ajellal N, Carpentier JF, Guillaume C, Guillaume SM, Helou M, Poirier V, Sarazin Y, Trifonov A. Dalton Trans. 2010;39:8363–8376. doi: 10.1039/c001226b. [DOI] [PubMed] [Google Scholar]
- [2d].Thomas CM, Lutz JF. Angew. Chem. 2011;123:9412–9414. [Google Scholar]; Angew. Chem. Int. Ed. 2011;50 [Google Scholar]
- [3a].Stanford MJ, Dove AP. Chem. Soc. Rev. 2010;39:486–494. doi: 10.1039/b815104k. [DOI] [PubMed] [Google Scholar]
- [3b].Dijkstra PJ, Du HZ, Feijen J. Polym. Chem. 2011;2:520–527. [Google Scholar]
- [3c].Buffet J-C, Okuda J. Polym. Chem. 2011;2:2758–2763. [Google Scholar]
- [4a].Ovitt TM, Coates GW. J. Am. Chem. Soc. 2002;124:1316–1326. doi: 10.1021/ja012052+. [DOI] [PubMed] [Google Scholar]
- [4b].Kakuta M, Hirata M, Kimura Y. Polym. Rev. 2009;49:107–140. [Google Scholar]
- [5a].Ikada Y, Jamshidi K, Tsuji H, Hyon SH. Macromolecules. 1987;20:904–906. [Google Scholar]
- [5b].Tsuji H, Ikada Y. Polymer. 1999;40:6699–6708. [Google Scholar]
- [5c].Tsuji H, Fukui I. Polymer. 2003;44:2891–2896. [Google Scholar]
- [6a].Jhurry D, Bhaw-Luximon A, Spassky N. Macromol. Symp. 2001;175:67–79. [Google Scholar]
- [6b].Nomura N, Ishii R, Akakura M, Aoi K. J. Am. Chem. Soc. 2002;124:5938–5939. doi: 10.1021/ja0175789. [DOI] [PubMed] [Google Scholar]
- [6c].Zhong ZY, Dijkstra PJ, Feijen J. Angew. Chem. 2002;114:4692–4695. [Google Scholar]; Angew. Chem. Int. Ed. 2002;41 [Google Scholar]
- [6d].Zhong Z, Dijkstra PJ, Feijen J. J. Am. Chem. Soc. 2003;125:11291–11298. doi: 10.1021/ja0347585. [DOI] [PubMed] [Google Scholar]
- [6e].Hormnirun P, Marshall EL, Gibson VC, White AJP, Williams DJ. J. Am. Chem. Soc. 2004;126:2688–2689. doi: 10.1021/ja038757o. [DOI] [PubMed] [Google Scholar]
- [6f].Majerska K, Duda A. J. Am. Chem. Soc. 2004;126:1026–1027. doi: 10.1021/ja0388966. [DOI] [PubMed] [Google Scholar]
- [6g].Hormnirun P, Marshall EL, Gibson VC, Pugh RI, White AJP. Proc. Natl. Acad. Sci. USA. 2006;103:15343–15348. doi: 10.1073/pnas.0602765103. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [6h].Du HZ, Pang X, Yu HY, Zhuang XL, Chen XS, Cui DM, Wang XH, Jing XB. Macromolecules. 2007;40:1904–1913. [Google Scholar]
- [6i].Nomura N, Ishii R, Yamamoto Y, Kondo T. Chem. Eur. J. 2007;13:4433–4451. doi: 10.1002/chem.200601308. [DOI] [PubMed] [Google Scholar]
- [6j].Bouyahyi M, Grunova E, Marquet N, Kirillov E, Thomas CM, Roisnel T, Carpentier JF. Organometallics. 2008;27:5815–5825. [Google Scholar]
- [6k].Alaaeddine A, Thomas CM, Roisnel T, Carpentier JF. Organometallics. 2009;28:1469–1475. [Google Scholar]
- [6l].Du H, Velders AH, Dijkstra PJ, Sun J, Zhong Z, Chen X, Feijen J. Chem. Eur. J. 2009;15:9836–9845. doi: 10.1002/chem.200900799. [DOI] [PubMed] [Google Scholar]
- [6m].Darensbourg DJ, Karroonnirun O. Organometallics. 2010;29:5627–5634. [Google Scholar]
- [6n].Bouyahyi M, Roisnel T, Carpentier J-F. Organometallics. 2012;31:1458–1466. [Google Scholar]
- [6o].Whitelaw EL, Loraine G, Mahon MF, Jones MD. Dalton Trans. 2011;40:11469–11473. doi: 10.1039/c1dt11438g. [DOI] [PubMed] [Google Scholar]
- [6p].Bakewell C, Platel RH, Cary SK, Hubbard SM, Roaf JM, Levine AC, White AJP, Long NJ, Haaf M, Williams CK. Organometallics. 2012;31:4729–4736. [Google Scholar]
- [6q].Chen H-L, Dutta S, Huang P-Y, Lin C-C. Organometallics. 2012;31:2016–2025. [Google Scholar]
- [6r].Bakewell C, White AJP, Long NJ, Williams CK. Inorg. Chem. 2013;52:12561–12567. doi: 10.1021/ic4016756. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [6s].Vieira ID, Whitelaw EL, Jones MD, Herres-Pawlis S. Chem. Eur. J. 2013;19:4712–4716. doi: 10.1002/chem.201203973. [DOI] [PubMed] [Google Scholar]
- [6t].Normand M, Dorcet V, Kirillov E, Carpentier JF. Organometallics. 2013;32:1694–1709. [Google Scholar]
- [6u].Hild F, Neehaul N, Bier F, Wirsum M, Gourlaouen C, Dagorne S. Organometallics. 2013;32:587–598. [Google Scholar]
- [6v].Hancock SL, Mahon MF, Jones MD. New J. Chem. 2013;37:1996–2001. [Google Scholar]
- [6w].Gao B, Duan RL, Pang X, Li X, Qu Z, Tang ZH, Zhuang XL, Chen XS. Organometallics. 2013;32:5435–5444. [Google Scholar]
- [6x].Cross ED, Allan LEN, Decken A, Shaver MP. J. Polym. Sci. Part A. 2013;51:1137–1146. [Google Scholar]
- [6y].Aluthge DC, Patrick BO, Mehrkhodavandi P. Chem. Commun. 2013;49:4295–4297. doi: 10.1039/c2cc33519k. [DOI] [PubMed] [Google Scholar]
- [6z].Pilone A, Press K, Goldberg I, Kol M, Mazzeo M, Lamberti M. J. Am. Chem. Soc. 2014;136:2940–2943. doi: 10.1021/ja412798x. [DOI] [PubMed] [Google Scholar]
- [7a].Zhang L, Nederberg F, Messman JM, Pratt RC, Hedrick JL, Wade CG. J. Am. Chem. Soc. 2007;129:12610–12611. doi: 10.1021/ja074131c. [DOI] [PubMed] [Google Scholar]
- [7b].Douglas AF, Patrick BO, Mehrkhodavandi P. Angew. Chem. 2008;120:2322–2325. doi: 10.1002/anie.200705033. [DOI] [PubMed] [Google Scholar]; Angew. Chem. Int. Ed. 2008;47 [Google Scholar]
- [7c].Yu I, Acosta-Ramirez A, Mehrkhodavandi P. J. Am. Chem. Soc. 2012;134:12758–12773. doi: 10.1021/ja3048046. [DOI] [PubMed] [Google Scholar]
- [7d].Horeglad P, Szczepaniak G, Dranka M, Zachara J. Chem. Commun. 2012;48:1171–1173. doi: 10.1039/c2cc16072b. [DOI] [PubMed] [Google Scholar]
- [7e].Fang J, Yu IS, Mehrkhodavandi P, Maron L. Organometallics. 2013;32:6950–6956. [Google Scholar]
- [7f].Gao B, Duan RL, Pang X, Li X, Qu Z, Shao HL, Wang XH, Chen XS. Dalton Trans. 2013;42:16334–16342. doi: 10.1039/c3dt52016a. [DOI] [PubMed] [Google Scholar]
- [8a].Arnold PL, Buffet J-C, Blaudeck RP, Sujecki S, Blake AJ, Wilson C. Angew. Chem. 2008;120:6122–6125. doi: 10.1002/anie.200801279. [DOI] [PubMed] [Google Scholar]; Angew. Chem. Int. Ed. 2008;47 [Google Scholar]
- [8b].Arnold PL, Buffet J-C, Blaudeck R, Sujecki S, Wilson C. Chem. Eur. J. 2009;15:8241–8250. doi: 10.1002/chem.200900522. [DOI] [PubMed] [Google Scholar]
- [8c].Bakewell C, Cao T-P-A, Long N, Le Goff XF, Auffrant A, Williams CK. J. Am. Chem. Soc. 2012;134:20577–20580. doi: 10.1021/ja310003v. [DOI] [PubMed] [Google Scholar]
- [8d].Bakewell C, Thi-Phuong-Anh C, Le Goff XF, Long NJ, Auffrant A, Williams CK. Organometallics. 2013;32:1475–1483. [Google Scholar]
- [9].Cordero B, Gomez V, Platero-Prats AE, Reves M, Echeverria J, Cremades E, Barragan F, Alvarez S. Dalton Trans. 2008:2832–2838. doi: 10.1039/b801115j. [DOI] [PubMed] [Google Scholar]
- [10a].Platel RH, Hodgson LM, Williams CK. Polym. Rev. 2008;48:11–63. [Google Scholar]
- [10b].Ma H, Spaniol TP, Okuda J. Dalton Trans. 2003:4770–4780. [Google Scholar]
- [10c].Cai CX, Amgoune A, Lehmann CW, Carpentier JF. Chem. Commun. 2004:330–331. doi: 10.1039/b314030j. [DOI] [PubMed] [Google Scholar]
- [10d].Amgoune A, Thomas CM, Roisnel T, Carpentier JF. Chem. Eur. J. 2006;12:169–179. doi: 10.1002/chem.200500856. [DOI] [PubMed] [Google Scholar]
- [10e].Liu X, Shang X, Tang T, Hu N, Pei F, Cui D, Chen X, Jing X. Organometallics. 2007;26:2747–2757. [Google Scholar]
- [10f].Ma H, Spaniol TP, Okuda J. Inorg. Chem. 2008;47:3328–3339. doi: 10.1021/ic702312b. [DOI] [PubMed] [Google Scholar]
- [10g].Grunova E, Kirillov E, Roisnel T, Carpentier JF. Dalton Trans. 2010;39:6739–6752. doi: 10.1039/b920283h. [DOI] [PubMed] [Google Scholar]
- [10h].Zhang Z, Cui D. Chem. Eur. J. 2011;17:11520–11526. doi: 10.1002/chem.201102074. [DOI] [PubMed] [Google Scholar]
- [10i].Zhang J, Qiu J, Yao Y, Zhang Y, Wang Y, Shen Q. Organometallics. 2012;31:3138–3148. [Google Scholar]
- [10j].Kratsch J, Kuzdrowska M, Schmid M, Kazeminejad N, Kaub C, Oña-Burgos P, Guillaume SM, Roesky PW. Organometallics. 2013;32:1230–1238. [Google Scholar]
- [11].Kowalski A, Duda A, Penczek S. Macromolecules. 1998;31:2114–2122. [Google Scholar]
- [12].Coudane J, Ustariz-Peyret C, Schwach G, Vert M. J. Polym. Sci. Part A. 1997;35:1651–1658. [Google Scholar]
- [13a].Ajellal N, Lyubov DM, Sinenkov MA, Fukin GK, Cherkasov AV, Thomas CM, Carpentier JF, Trifonov AA. Chem. Eur. J. 2008;14:5440–5448. doi: 10.1002/chem.200800288. [DOI] [PubMed] [Google Scholar]
- [13b].Wang Y, Luo Y, Chen J, Xue H, Liang H. New J. Chem. 2012;36:933–940. [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.