Abstract

Ni-rich LiNi0.8Co0.1Mn0.1O2 layered oxide cathodes have been highlighted for large-scale energy applications due to their high energy density. Although its specific capacity is enhanced at higher voltages as Ni ratio increases, its structural degradation due to phase transformations and lattice distortions during cycling becomes severe. For these reasons, we focused on the origins of crack generation from phase transformations and structural distortions in Ni-rich LiNi0.8Co0.1Mn0.1O2 using multiscale approaches, from first-principles to meso-scale phase-field model. Atomic-scale structure analysis demonstrated that opposite changes in the lattice parameters are observed until the inverse Li content x = 0.75; then, structure collapses due to complete extraction of Li from between transition metal layers. Combined-phase investigations represent the highest phase barrier and steepest chemical potential after x = 0.75, leading to phase transformations to highly Li-deficient phases with an inactive character. Abrupt phase transformations with heterogeneous structural collapse after x = 0.81 (~220 mAh g−1) were identified in the nanodomain. Further, meso-scale strain distributions show around 5% of anisotropic contraction with lower critical energy release rates, which cause not only micro-crack generations of secondary particles on the interfaces between the contracted primary particles, but also mechanical instability of primary particles from heterogeneous strain changes.


Ni-rich transition metal layered oxides (LiNixCoyMn1−xyO2, with x > 0.5, Ni-rich NCM) have been spotlighted during the past decade as the most promising candidates for high capacity cathode materials in Li-ion batteries (LIBs) due to their high energy densities (>200 mAh g−1 until ~4.6 V vs. Li/Li+)1,2,3. Although LiNi1/3Co1/3Mn1/3O2 (NCM111) has been successfully commercialized, in order to meet the demand for large-scale energy storage applications such as electric vehicles (EVs) and energy storage systems (ESSs), further NCM research and development have been directed toward enhancing its specific capacity by increasing the ratio of the Ni component toward LiNi0.8Co0.1Mn0.1O2 (NCM811)4,5,6.

While the increase of the Ni ratio in NCM contributes to an enhanced specific discharge capacity, it also results in severe capacity degradation caused by cation mixing, surface side reactions, and crack propagation with structural instability1. To better understand these challenges, Jung et al. investigated the degradation mechanism of the phase transformation induced by cation mixing from the surface to bulk using ex situ structural analysis7. Similarly, Lin et al. described the surface reconstruction and chemical evolution of the rhombohedral layered structure to a cubic spinel structure using high-throughput X-ray absorption spectroscopy8. As theoretical approaches, electronic correlations for the redox reactions between the multivalent transition metals in the Ni-rich NCM9 and stability analysis with respect to the various ratios of the Ni, Co, and Mn components in the NCM10 have been performed through first-principles calculations. On the bases of these fundamental data, many researchers have suggested solutions to resolve the cyclic degradation problem. Along with diverse approaches such as morphology control11, elemental doping12,13,14,15 and surface coating16,17,18,19,20, Sun et al. have suggested various effective ways to reduce cyclic degradation and improve electrochemical performance through the design of core-shell21, gradient core-shell3,22, and full concentration gradient structures2,23,24 for Ni-rich NCM cathodes.

Nevertheless, micro-crack propagation in the secondary particle related to structural instability remains problematic, although cation mixing and surface deterioration can be prevented through the above-mentioned approaches. Among the promising Ni-rich compounds, severe structural changes and crack propagation have been observed experimentally in LiNixCoyAl1−xyO2 (NCA) cathodes25,26,27,28. Although, Meng et al. recently reported the experimental observation of micro-crack generation of NCM811 with severe cyclic degradation and suggested surface coating with Li2TiO3 to mitigate the crack propagation29, the fundamental origin has not been adequately addressed for the Ni-rich NCM cathodes1. Moreover, the underlying mechanism for the phase transformation and structural changes in NCM811 is not fully understood. For these reasons, we focused on the study of intrinsic characteristics of the phase transformation and structural changes of NCM811 to elucidate its inherent structural instability regardless of cation mixing and surface deterioration.

Through multiscale phase-transformation mechanics based on first-principles calculations, here, we investigated the fundamental reaction mechanism, structural distortions, thermodynamic combined-phase (CP) behaviours, and meso-scale phase-separation kinetics for NCM811 with respect to varying Li concentration. Since the redox reactions during cycling mainly involve the Ni and O ions, the Co and Mn ions would retain similar electronic structures before and after delithiation. Anisotropic structural changes are observed between the ab plane and c axis, which result in anisotropic shrinkage of the entire structure. In particular, an abrupt collapse of the structure is observed for an inverse Li content x = 0.75–1.0 in Li1−xNi0.8Co0.1Mn0.1O2. The CP behaviour shows generally one-phase reactions with lower phase barriers below x = 0.75. However, a two-phase region with a remarkably higher phase barrier is presented after x = 0.75 and inactive phases are formed, which not only agrees well with the experiments of Ohzuku et al30. but also correlates with the collapse of the structure after x = 0.75. Based on these first-principles calculation results, meso-scale phase separation simulations were performed, which reveals heterogeneous phase transformations and structural changes at different Li concentrations. Therefore, an intrinsic limitation of NCM811 exists in the region x = 0.75–0.81 (~220 mAh g−1) due to the inactive phase separation and abrupt structural changes. Around 5% of the anisotropic contraction was observed in the nanodomain, which induces the contractions of the primary particles. In addition, very low critical energy release rates for crack generation of fully-lithiated and delithiated NCM811 were calculated. Such large volume reduction and low critical energy release rate could be the reason of causing the micro-crack generations in the secondary particles on the interfaces between the contracted primary particles. Further, the heterogeneous strain changes cause severe mechanical instability within the primary particles, which could be the reason of the generation of nano-cracks as a seed of the micro-cracks. These findings should provide helpful insights for the development of Ni-rich NCM cathode materials in the Li-ion battery research community.

Results and Discussion

Redox Mechanism and Structural distortion

Figure 1a and b show the atomic model used for the first-principles calculations projected on the bc and ab planes, respectively. The atomic model was developed based on the rhombohedral layered oxide structure (R-3m) of LiNiO2 (Inorganic Crystal Structure Database (ICSD) ID: 10499). To represent the stoichiometry of NCM811, supercells of 2 × 2 × 1 with 12f.u. were used; the exact stoichiometry of the supercell in this study is LiNi0.8333Co0.0833Mn0.0833O2 (Li12Ni10Co1Mn1O24). The model was developed using high-throughput calculations based on previously described schemes31,32,33,34,35. As shown in Fig. 1a, Co and Mn are located separately in the Ni-rich environment of the layered oxide structure, which would be thermodynamically related to d-electronic stability of the crystal field36,37.

Figure 1.

Figure 1

Atomic models of Ni-rich LiNi0.8Co0.1Mn0.1O2 (NCM811) layered oxide (R-3m) projected onto the (a) bc and (b) ab planes.

Figure 2 presents the partial (projected) density of states (PDOSs) of the Ni, Co, and Mn d-orbitals and the O p-orbitals in Li1Ni0.8Co0.1Mn0.1O2 and Li0Ni0.8Co0.1Mn0.1O2 (Fig. 2a–d and 2e–h, respectively). In the fully lithiated state (Li1Ni0.8Co0.1Mn0.1O2), the Ni, Co, and Mn d-orbitals are shown as Ni3-like, Co3+, and Mn4+-like shapes due to the effect of the d-electronic donor9,38, in agreement with a previous report10. The thermodynamic stability of the Co3+ and Mn4+ crystal fields could be satisfied by maintaining their separate locations. Based on the electronic structures, further, the redox reactions of NCM811 can be understood. Fig. 2e–h present the PDOSs of the fully delithiated state (Li0Ni0.8Co0.1Mn0.1O2). The charts reveal Ni4+, Co3+, and Mn4+-like shapes, which indicate that the cationic redox reaction of Ni3+-like to Ni4+ is a major cationic redox process. Additionally, Fig. 2d and 2h indicate a notable anionic redox reaction contribution from O ions. Therefore, the superior electrochemical performance of the Ni-rich NCM can be attributed to the combination of the anionic redox reactions39,40 and the cationic redox reactions of the Ni ions in the stable crystal fields of the Co and Mn d-orbitals.

Figure 2.

Figure 2

(a,b,c,d) Partial density of states (PDOSs) of (a) Ni d- (gray solid line), (b) Co d- (blue solid line), (c) Mn d- (purple solid line), and (d) O p- (red solid line) orbitals in LiNi0.8Co0.1Mn0.1O2. (e,f,g,h) PDOSs of (e) Ni d- (gray dashed line), (f) Co d- (blue dashed line), (g) Mn d- (purple dashed line), and (h) O p- (red dashed line) orbitals in Li0.0Ni0.8Co0.1Mn0.1O2. The Fermi level is 0.0 eV (green dotted line).

From a structural point of view, NCM811 suffers from severe structural changes with anisotropic distortions. Figure 3a shows the expansion and contraction of the a (blue left axis) and c (red right axis) lattice parameters as a function of the inverse Li content x in Li1−xNi0.8Co0.1Mn0.1O2. In the a direction, the lattice decreases gradually throughout the reaction from x = 0 to 1, whereas the lattice in the c direction shows non-monotonic behaviour, increasing from x = 0.0 to 0.75 and decreasing thereafter. In other words, the lattice parameters change in opposite directions from x = 0.0 to 0.75, but in the same direction thereafter. However, after x = 0.75, structural collapse is observed due to the rapid volume reduction, as shown in Fig. 3b, which is caused by the complete extraction of Li ions from between the transition metal layers. Therefore, the structural changes of NCM811 during electrochemical reactions are likely to be harmful to the cyclic performance due to the lattice distortions in opposing directions (0.0 < x < 0.75) and the volumetric collapse (0.75 < x < 1.0).

Figure 3.

Figure 3

(a) Calculated a (blue inverse triangles and solid line, left axis) and c lattice parameters (red triangles and solid line, right axis), and (b) volume of cell (black circles and solid line) with respect to the inverse Li content x in Li1−xNi0.8Co0.1Mn0.1O2.

Heterogeneous Phase Transformation

To understand the thermodynamic phase transformations, the phase behaviours were investigated by calculating the DFT mixing enthalpies HDFT(x) with respect to normalized inverse Li content x using Eq. (1), as presented in Fig. 4a. Seven ground states are observed, including the initial (x = 0) and final (x = 1) states. The CP redox reaction of NCM811 consists of two one-phase reactions (0.0 < x < 0.1667; 0.3333 < x < 0.4167) and three two-phase reactions (0.1667 < x < 0.3333; 0.4167 < x < 0.75; 0.75 < x < 1.0). To predict the electrochemical behaviour, Fig. 4b presents the OCVs based on the ground states in Fig. 4a; the shape of the curve is similar to the experimental OCV values for LiNiO2 estimated previously by the galvanostatic intermittent titration technique (GITT)30.

Figure 4.

Figure 4

(a) Mixing enthalpies from density functional theory (DFT) calculations (black circles) with ground states (yellow diamonds and blue line). (b) Open-circuit voltage (OCV) calculated using first principles (blue solid line) and reproduced by experiment (black circles and line) from Ohzuku et al30. versus inverse Li content x in Li1−xNi0.8Co0.1Mn0.1O2.

By considering the configurational entropy at a finite temperature (300 K), more general phase behaviours can be understood using the CP free energy fCP(x) and the CP chemical potential μCP of Eqs (2) and (3), as shown in Fig. 5. Spinodal regions, where two-phase reactions occur, are indicated as green shaded regions in Fig. 5. Figure 5a shows that the first and second phase barriers from x = 0.21 to 0.30 and from x = 0.50 to 0.67 are low, but the third phase barrier from x = 0.81 to 0.93 is remarkably steep and higher than the others. This means that phase separations are likely to be impeded due to the low phase barriers and the low slopes of the chemical potentials before x = 0.75, such that relatively smooth reactions similar to the one-phase reaction can be generated, rather than the two-phase reaction. In contrast, after x = 0.75, rapid phase separation by a two-phase reaction is likely to occur as indicated by the higher phase barrier in Fig. 5a and the sharp slope of the chemical potential in Fig. 5b. More importantly, the strong phase separation after x = 0.75 results in a highly Li-deficient phase (Li0Ni0.8Co0.1Mn0.1O2), leading to severe structural transformations to inactive phases such as the NiO rock salt phase previously observed by ex situ transmission electron microscopy in Ni-rich NCM7.

Figure 5.

Figure 5

(a) Combined-phase (CP) free energy (blue solid line) and (b) CP chemical potential (red solid line) at room temperature (300 K) with spinodal regions (green shaded areas) with respect to inverse Li content x in Li1-xNi0.8Co0.1Mn0.1O2.

Origins of Crack Generation

To describe the meso-scale phase transformations of LiNi0.8Co0.1Mn0.1O2 in a nanodomain with dimensions of 31.36 nm × 31.36 nm at 300 K, a phase-field model analysis was conducted by solving Eqs (9) and (10). As simulation parameters, we set D as 10−8 cm2 s−1 based on an experimental value41, λ as 0.49 nm from the interlayer distance of the atomic model, and the Inline graphic values as Inline graphic = 128.66 eV, Inline graphic = 7.85 eV, and Inline graphic = 169.95 eV. The phase transformation simulations were carried out on the ac plane during relaxation from the solid solution at x = 0.65 (Fig. 6a) with a theoretical charge capacity of ~179 mAh g−1 and x = 0.85 (Fig. 6e) with a theoretical charge capacity of ~234 mAh g−1. The a, c, and volumetric strains (denoted as ε1, ε3, and εV, respectively) are displayed in Fig. 6b (x = 0.65) and f (x = 0.85), 6c (x = 0.65) and 6g(x = 0.85), and 6d (x = 0.65) and 6h(x = 0.85), respectively. The strains are defined as ε1 = Δa/ax = 0, ε3 = Δc/cx=0, and εV = ΔV/Vx=0, where a and c are the lattice parameters and V is the volume, respectively. Finally, 2D diffusion in the a and b directions was applied, and the phase separation was triggered by random noise.

Figure 6.

Figure 6

Meso-scale phase transformations in the nanodomain with dimensions of 31.36 × 31.36 nm in Li1−xNi0.8Co0.1Mn0.1O2 at room temperature (300 K) from a solid solution of inverse Li concentration x = 0.65 (a,b,c,d) and 0.85 (e,f,g,h) at dimensionless time Inline graphic = 5. (a,e), (b,f), (c,g), and (d,h) are the distributions on the ac plane of the inverse Li concentration x, strain in a direction ε1, strain in c direction ε3, and volumetric strain εV, respectively.

From the distribution of the inverse Li concentration, distinct phase separation is observed in Fig. 6e at x = 0.85, correlated with the sharp slope of the chemical potential in Fig. 5b, but only slight phase separation is observed in Fig. 6a at x = 0.65. For this reason, smooth electrochemical reactions may be possible until x = 0.65 (~179 mAh g−1), but phase separation to an inactive phase (Li0Ni0.8Co0.1Mn0.1O2) should occur at x = 0.85 (~234 mAh g−1), meaning that the third spinodal region from x = 0.81 to 0.93 induces intrinsically irreversible characteristics. Furthermore, from a structural perspective, at x = 0.65, not only are contraction strains of ε1 and ε3 observed, but also slight differences occur between ε1 (–6 × 10−6 < ε1 < –6 × 10−7) and ε3 (0.027 < ε3 < 0.028), as shown in Fig. 6b and c. Fortunately, the extent of structural change can be considered as reasonably small; e.g., the difference in εV is less than 4 × 10−4, as illustrated in Fig. 6d. Severe structural distortions occur at x = 0.85. All the absolute changes in the three strains at x = 0.85 are remarkably larger than those at x = 0.65: ε1 changes relatively slightly (–0.032 < ε1 < –0.027), whereas ε3 and εV vary by as much as 5% (0.018 < ε3 < 0.043, –0.047 < εV < –0.018) (Fig. 6f,g and h, respectively). Videos attached in the supplementary information illustrate the specific evolution of the inverse concentration of Li and the volumetric strain.

In the meso-scale phase transformation phenomena, the structural distortions are heterogeneously generated in the nanodomain due to the blocking of diffusion in the c direction and the rapid phase separation, which is shown in the apparent red and blue regions of Fig. 6f,g and h. Therefore, the structural changes in NCM811 occur more severely in the third spinodal region, and, combined with the abrupt phase separation, limit the intrinsic specific capacity to less than 220 mAh g−1 for x = 0.81. As shown in Fig. 7, the around 5% of anisotropic contraction and the ~3.9% of average contraction (Fig. 6h) in the nanodomain would cause the contraction of each primary particle, and then the gaps between the primary particles would result in the micro-crack generations in the secondary particles on the interfaces between the primary particles, which could be the origins and mechanism on the experimental observations of the micro-crack propagations25,26,27,28,29. Further, the heterogeneous distribution of the anisotropic strain changes causes the severe mechanical instability of the primary particles that could induce the generation of nano-cracks, which could be a crack opening of the micro-cracks.

Figure 7. Schematic illustration of micro-crack generations in secondary particles on the interfaces of the contracted primary particles during delithiation.

Figure 7

In addition, Table 1 shows critical energy release rates of Li1Ni0.8Co0.1Mn0.1O2 and Li0Ni0.8Co0.1Mn0.1O2 calculated by DFT, which describe the critical energy for the crack generation and are related to the surface energy γ for brittle materials (Gc = 2γ) based on Griffith’s theory. Though fully-lithiated NCM811 has low Gc (2.4308 J m−2), the delithiated NCM811 has even lower Gc (−0.0064 J m−2), which would result from the structural instability between layers at lower Li concentrations. In other words, not only NCM811 is fragile to crack generation, but also it gets weakened at delithiated states, which means the 5% of anisotropic contraction could be enough to generate crack propagations.

Table 1. Critical energy release rates Gc for a crack generation of Li1Ni0.8Co0.1Mn0.1O2 and Li0Ni0.8Co0.1Mn0.1O2 based on Griffith’s theory.

  Li1Ni0.8Co0.1Mn0.1O2 Li0Ni0.8Co0.1Mn0.1O2
Gc 2.4308 J m−2 −0.0064 J m−2

Recently, Meng et al. reported that the severe crack generation in NCM811 particles induces a significant performance degradation29. According to the scanning electron microscopy (SEM) observation, particle fractures and fragmentation of NCM811 particles were evident after cycles. Due to this crack generation, the discharge capacity of NCM811 was remarkably decreased with increasing overpotentials during cycles. From our fundamental understanding, we suggest that the origin of crack generation is the contraction of primary particles with a mechanical instability caused by heterogeneous phase transformation and anisotropic strain changes. In addition, the lower Gc at delithiated states contributes to a severe crack propagation. Finally, it is expected that these could be resolved by reducing the inhomogeneity and anisotropy of structural changes and increasing Gc.

Conclusion

The intrinsic limitations of a Ni-rich NCM811 cathode material were investigated in terms of its phase transformations and structural distortions using multiscale approaches combining first-principles calculations and the CP phase-field model. The major redox mechanism of NCM811 was determined as a combination of the cationic redox reactions of Ni with the anionic redox reactions of O. The atomic-scale structural analysis showed that opposite lattice changes are generated until x = 0.75, followed thereafter by the gradual decrease all of the lattice parameters due to the collapse of the transition metal layers. The CP behaviours represent the three two-phase reaction regions, wherein the third exhibits a higher phase barrier and a sharp rise in the chemical potential. This causes rapid phase separation, forming an inactive and highly Li-deficient phase. In the meso-scale phase transformation, heterogeneous phase separations are observed, and severe phase transformation occurs near the third spinodal region at x = 0.85. Further, the ~3.9% of the average contraction and lower critical energy release rates including the heterogeneous distribution of the anisotropic strain changes observed by the meso-scale strain distributions could induce not only the nano-cracks in the nanodomain of the primary particles from the severe mechanical instability, but also the micro-crack generations on the interfaces between the contracted primary particles. Thus, the combination of the abrupt transformations to inactive phases with the heterogeneous collapse of the layered structure limits the intrinsic performance of NCM811. These findings may help to predict the maximum performance of Ni-rich NCM cathodes, and the mechanistic insights on the phase transformations and structural distortions could provide clues toward improving cathode materials for battery applications.

Methodology

First-principles calculations

For the atomic-scale simulations, first-principles calculations were conducted using spin-polarized density functional theory (DFT) with the generalized gradient approximation (GGA) according to the Perdew-Wang 91 exchange-correlation functional42. The Vienna Ab Initio Simulation Package (VASP) was utilized to implement a plane-wave basis set and the projector-augmented wave (PAW) method43,44. To evaluate accurate electrochemical and d-orbital electronic properties, the Hubbard U parameter was used45. The U values for Ni, Co, and Mn (6.7, 4.91, and 4.64, respectively) were chosen from previous reports37,46. As computational parameters, a plane-wave cut-off energy of 500 eV and k-point meshes of 4 × 4 × 2 for the Brillouin zone sampling were determined by a convergence test. The atomic model for NCM811 was developed by the 12 formula units (f.u.) of LiNi0.8333Co0.0833Mn0.0833O2 using high-throughput calculations31,32,33,34,35. All the calculations were based on fully relaxed structures.

Combined-phase (CP) phase transformation mechanics

For the multiscale analyses from the atomic- to meso-scale, we adopted the CP transformation model47,48 and the Cahn-Hilliard equation49.

First, the DFT mixing enthalpy HDFT(x) with respect to the normalized inverse Li content x from 0.0 to 1.0 for battery electrodes can be defined as follows:

graphic file with name srep39669-m5.jpg

where Inline graphic represents the total energy of Li1−xNi0.8Co0.1Mn0.1O2 as calculated from DFT calculations. From the convex hull analysis of HDFT(x), the CP free energy fCP(x) and the CP chemical potential μCP at finite temperature by considering the configurational entropy50 can be determined based on the CP mixing enthalpy HCP(x) as follows:

graphic file with name srep39669-m7.jpg
graphic file with name srep39669-m8.jpg
graphic file with name srep39669-m9.jpg

where, kB and T represent the Boltzmann constant and absolute temperature, respectively. Furthermore, the enthalpy coefficient Inline graphic in the reaction regions from xi to xf is obtained by parameterization from the CP mixing enthalpy Inline graphic as follows:

graphic file with name srep39669-m12.jpg

The open-circuit voltage (OCV) VDFT was calculated using DFT at 0 K as follows:

graphic file with name srep39669-m13.jpg

To solve the meso-scale phase transformation phenomena, the CP Cahn-Hilliard energy function GCP was defined as follows:

graphic file with name srep39669-m14.jpg

where, ρn represents the number of sites per volume V and Inline graphic is the gradient energy coefficient determined by the characteristic length λ and enthalpy coefficient Inline graphic as follows:51,52

graphic file with name srep39669-m17.jpg

We applied the semi-implicit Fourier-spectral method53 with a periodic boundary condition (PBC) to compute the Cahn-Hilliard equation49. For non-dimensionalization, kBT, λ, and D/λ2 were used as the dimensionless energy, length, and time scales with the use of the diffusion coefficient D, respectively. Based on these dimensionless parameters, the Cahn-Hilliard equation can be written as follows:

graphic file with name srep39669-m18.jpg

Then, Eq. (9) can be re-written on the Fourier space with a wave vector k as follows:

graphic file with name srep39669-m19.jpg

Additional Information

How to cite this article: Lim, J.-M. et al. Intrinsic Origins of Crack Generation in Ni-rich LiNi0.8Co0.1Mn0.1O2 layered oxide cathode material. Sci. Rep. 7, 39669; doi: 10.1038/srep39669 (2017).

Publisher's note: Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Supplementary Material

Supplementary Information
srep39669-s1.doc (45.5KB, doc)
Supplementary Video 1
Download video file (145.8KB, avi)
Supplementary Video 2
Download video file (330.6KB, avi)
Supplementary Video 3
Download video file (279.3KB, avi)
Supplementary Video 4
Download video file (347.7KB, avi)

Acknowledgments

This study was supported by a National Research Foundation of Korea (NRF) grant funded by the Korean government (MEST) (2012R1A3A2048841), as well as by the New & Renewable Energy Core Technology Program (No. 20152020105420) funded by the Ministry of Trade, Industry & Energy (MOTIE), Republic of Korea. Computational resources for the high-throughput calculations were supported by the iBAT platform of the Industrial Strategic Technology Development Program (Grant No. 10041589) funded by MOTIE, Republic of Korea. This work was also supported by the R&D Programs of National Research Council of Science & Technology (Project No. CAP-14-2-KITECH).

Footnotes

Author Contributions M.C. and J.M.L. conceived and designed this work. J.M.L., D.K. and T.H. performed the first-principles calculations. J.M.L. carried out the multiscale phase field simulations and calculated strain distributions with critical energy release rates. M.C., M.S.P., and K.C. supervised this study. M.C., K.C., M.S.P., and J.M.L. wrote the paper. All authors reviewed the manuscript.

References

  1. Liu W. et al. Nickel-rich layered lithium transition-metal oxide for high-energy lithium-ion batteries. Angew Chem Int Ed Engl 54, 4440–4457, doi: 10.1002/anie.201409262 (2015). [DOI] [PubMed] [Google Scholar]
  2. Sun Y. K. et al. Nanostructured high-energy cathode materials for advanced lithium batteries. Nat Mater 11, 942–947, doi: 10.1038/nmat3435 (2012). [DOI] [PubMed] [Google Scholar]
  3. Sun Y. K. et al. High-energy cathode material for long-life and safe lithium batteries. Nat Mater 8, 320–324, doi: 10.1038/nmat2418 (2009). [DOI] [PubMed] [Google Scholar]
  4. Armand M. & Tarascon J. M. Building better batteries. Nature 451, 652–657, doi: 10.1038/451652a (2008). [DOI] [PubMed] [Google Scholar]
  5. Dunn B., Kamath H. & Tarascon J. M. Electrical Energy Storage for the Grid: A Battery of Choices. Science 334, 928–935, doi: 10.1126/science.1212741 (2011). [DOI] [PubMed] [Google Scholar]
  6. Manthiram A., Knight J. C., Myung S.-T., Oh S.-M. & Sun Y.-K. Nickel-Rich and Lithium-Rich Layered Oxide Cathodes: Progress and Perspectives. Advanced Energy Materials 6, 1501010, doi: 10.1002/aenm.201501010 (2016). [DOI] [Google Scholar]
  7. Jung S.-K. et al. Understanding the Degradation Mechanisms of LiNi0.5Co0.2Mn0.3O2Cathode Material in Lithium Ion Batteries. Advanced Energy Materials 4, 1300787, doi: 10.1002/aenm.201300787 (2014). [DOI] [Google Scholar]
  8. Lin F. et al. Surface reconstruction and chemical evolution of stoichiometric layered cathode materials for lithium-ion batteries. Nat Commun 5, 3529, doi: 10.1038/ncomms4529 (2014). [DOI] [PubMed] [Google Scholar]
  9. Kim D. et al. Design of Nickel-rich Layered Oxides UsingdElectronic Donor for Redox Reactions. Chemistry of Materials 27, 6450–6456, doi: 10.1021/acs.chemmater.5b02697 (2015). [DOI] [Google Scholar]
  10. Liang C. et al. Unraveling the Origin of Instability in Ni-Rich LiNi1–2xCoxMnxO2(NCM) Cathode Materials. The Journal of Physical Chemistry C 120, 6383–6393, doi: 10.1021/acs.jpcc.6b00369 (2016). [DOI] [Google Scholar]
  11. Chen Z. et al. Hierarchical Porous LiNi1/3Co1/3Mn1/3O2 Nano-/Micro Spherical Cathode Material: Minimized Cation Mixing and Improved Li(+) Mobility for Enhanced Electrochemical Performance. Sci Rep 6, 25771, doi: 10.1038/srep25771 (2016). [DOI] [PMC free article] [PubMed] [Google Scholar]
  12. Yu Z. et al. Ti-substituted Li[Li0.26Mn0.6−xTixNi0.07Co0.07]O2layered cathode material with improved structural stability and suppressed voltage fading. J. Mater. Chem. A 3, 17376–17384, doi: 10.1039/c5ta03764f (2015). [DOI] [Google Scholar]
  13. Conry T. E., Mehta A., Cabana J. & Doeff M. M. Structural Underpinnings of the Enhanced Cycling Stability upon Al-Substitution in LiNi0.45Mn0.45Co0.1-yAlyO2 Positive Electrode Materials for Li-ion Batteries. Chemistry of Materials 24, 3307–3317, doi: 10.1021/cm3011937 (2012). [DOI] [Google Scholar]
  14. Luo W. B., Li X. H. & Dahn J. R. Synthesis, Characterization, and Thermal Stability of Li[Ni1/3Mn1/3Co1/3-z(MnMg)(z/2)]O-2. Chemistry of Materials 22, 5065–5073, doi: 10.1021/cm1017163 (2010). [DOI] [Google Scholar]
  15. Tatsumi K. et al. Local atomic and electronic structures around Mg and Al dopants in LiNiO2 electrodes studied by XANES and ELNES and first-principles calculations. Phys Rev B 78, doi: ARTN 04510810.1103/PhysRevB.78.045108 (2008). [Google Scholar]
  16. Cho J., Kim T.-J., Kim J., Noh M. & Park B. Synthesis, Thermal, and Electrochemical Properties of AlPO[sub 4]-Coated LiNi[sub 0.8]Co[sub 0.1]Mn[sub 0.1]O[sub 2] Cathode Materials for a Li-Ion Cell. Journal of The Electrochemical Society 151, A1899, doi: 10.1149/1.1802411 (2004). [DOI] [Google Scholar]
  17. Lee Y. S., Ahn D., Cho Y. H., Hong T. E. & Cho J. Improved Rate Capability and Thermal Stability of LiNi0.5Co0.2Mn0.3O2 Cathode Materials via Nanoscale SiP2O7 Coating. Journal of the Electrochemical Society 158, A1354–A1360, doi: 10.1149/2.051112jes (2011). [DOI] [Google Scholar]
  18. Cho Y., Oh P. & Cho J. A New Type of Protective Surface Layer for High-Capacity Ni-Based Cathode Materials: Nanoscaled Surface Pillaring Layer. Nano Lett 13, 1145–1152, doi: 10.1021/nl304558t (2013). [DOI] [PubMed] [Google Scholar]
  19. Jo C. H. et al. An effective method to reduce residual lithium compounds on Ni-rich Li[Ni0.6Co0.2Mn0.2]O-2 active material using a phosphoric acid derived Li3PO4 nanolayer. Nano Res 8, 1464–1479, doi: 10.1007/s12274-014-0631-8 (2015). [DOI] [Google Scholar]
  20. Mohanty D. et al. Modification of Ni-Rich FCG NMC and NCA Cathodes by Atomic Layer Deposition: Preventing Surface Phase Transitions for High-Voltage Lithium-Ion Batteries. Sci Rep 6, 26532, doi: 10.1038/srep26532 (2016). [DOI] [PMC free article] [PubMed] [Google Scholar]
  21. Sun Y. K., Myung S. T., Kim M. H., Prakash J. & Amine K. Synthesis and characterization of Li[(Ni0.8Co0.1Mn0.1)(0.8)(Ni0.5Mn0.5)(0.2)]O-2 with the microscale core-shell structure as the positive electrode material for lithium batteries. J Am Chem Soc 127, 13411–13418, doi: 10.1021/ja053675g (2005). [DOI] [PubMed] [Google Scholar]
  22. Sun Y.-K., Kim D.-H., Jung H.-G., Myung S.-T. & Amine K. High-voltage performance of concentration-gradient Li[Ni0.67Co0.15Mn0.18]O2 cathode material for lithium-ion batteries. Electrochimica Acta 55, 8621–8627, doi: 10.1016/j.electacta.2010.07.074 (2010). [DOI] [Google Scholar]
  23. Li Y. et al. Synthesis of full concentration gradient, cathode studied by high energy X-ray diffraction. Nano Energy 19, 522–531, doi: 10.1016/j.nanoen.2015.07.019 (2016). [DOI] [Google Scholar]
  24. Park K. J. et al. A high-capacity Li[Ni0.8Co0.06Mn0.14]O-2 positive electrode with a dual concentration gradient for next-generation lithium-ion batteries. J Mater Chem A 3, 22183–22190, doi: 10.1039/c5ta05657h (2015). [DOI] [Google Scholar]
  25. Huang R. & Ikuhara Y. STEM characterization for lithium-ion battery cathode materials. Current Opinion in Solid State and Materials Science 16, 31–38, doi: 10.1016/j.cossms.2011.08.002 (2012). [DOI] [Google Scholar]
  26. Miller D. J., Proff C., Wen J. G., Abraham D. P. & Bareño J. Observation of Microstructural Evolution in Li Battery Cathode Oxide Particles by In Situ Electron Microscopy. Advanced Energy Materials 3, 1098–1103, doi: 10.1002/aenm.201300015 (2013). [DOI] [Google Scholar]
  27. Zheng S. et al. Microstructural Changes in LiNi0.8Co0.15Al0.05O2 Positive Electrode Material during the First Cycle. Journal of The Electrochemical Society 158, A357, doi: 10.1149/1.3544843 (2011). [DOI] [Google Scholar]
  28. Watanabe S., Kinoshita M., Hosokawa T., Morigaki K. & Nakura K. Capacity fade of LiAlyNi1-x-yCoxO2 cathode for lithium-ion batteries during accelerated calendar and cycle life tests (surface analysis of LiAlyNi1-x-yCoxO2 cathode after cycle tests in restricted depth of discharge ranges). Journal of Power Sources 258, 210–217, doi: 10.1016/j.jpowsour.2014.02.018 (2014). [DOI] [Google Scholar]
  29. Meng K., Wang Z., Guo H., Li X. & Wang D. Improving the cycling performance of LiNi0.8Co0.1Mn0.1O2 by surface coating with Li2TiO3. Electrochimica Acta 211, 822–831, doi: 10.1016/j.electacta.2016.06.110 (2016). [DOI] [Google Scholar]
  30. Ohzuku T., Ueda A. & Nagayama M. Electrochemistry and Structural Chemistry of Linio2 (R(3)over-Bar-M) for 4 Volt Secondary Lithium Cells. Journal of the Electrochemical Society 140, 1862–1870, doi: 10.1149/1.2220730 (1993). [DOI] [Google Scholar]
  31. Hautier G. et al. Novel mixed polyanions lithium-ion battery cathode materials predicted by high-throughput ab initio computations. J Mater Chem 21, 17147–17153, doi: 10.1039/c1jm12216a (2011). [DOI] [Google Scholar]
  32. Hautier G. et al. Phosphates as Lithium-Ion Battery Cathodes: An Evaluation Based on High-Throughput ab Initio Calculations. Chemistry of Materials 23, 3495–3508, doi: 10.1021/cm200949v (2011). [DOI] [Google Scholar]
  33. Jain A., Hautier G., Ong S. P., Dacek S. & Ceder G. Relating voltage and thermal safety in Li-ion battery cathodes: a high-throughput computational study. Phys Chem Chem Phys 17, 5942–5953, doi: 10.1039/c5cp00250h (2015). [DOI] [PubMed] [Google Scholar]
  34. Morgan D., Ceder G. & Curtarolo S. High-throughput and data mining with ab initio methods. Meas Sci Technol 16, 296–301, doi: 10.1088/0957-0233/16/1/039 (2005). [DOI] [Google Scholar]
  35. Mueller T., Hautier G., Jain A. & Ceder G. Evaluation of Tavorite-Structured Cathode Materials for Lithium-Ion Batteries Using High-Throughput Computing. Chemistry of Materials 23, 3854–3862, doi: 10.1021/cm200753g (2011). [DOI] [Google Scholar]
  36. Lim J.-M. et al. The origins and mechanism of phase transformation in bulk Li2MnO3: first-principles calculations and experimental studies. J Mater Chem A 3, 7066–7076, doi: 10.1039/c5ta00944h (2015). [DOI] [Google Scholar]
  37. Lim J. M., Kim D., Park M. S., Cho M. & Cho K. Underlying mechanisms of the synergistic role of Li2MnO3 and LiNi1/3Co1/3Mn1/3O2 in high-Mn, Li-rich oxides. Phys Chem Chem Phys 18, 11411–11421, doi: 10.1039/c6cp00088f (2016). [DOI] [PubMed] [Google Scholar]
  38. Kang K. S., Meng Y. S., Breger J., Grey C. P. & Ceder G. Electrodes with high power and high capacity for rechargeable lithium batteries. Science 311, 977–980, doi: 10.1126/science.1122152 (2006). [DOI] [PubMed] [Google Scholar]
  39. Grimaud A., Hong W. T., Shao-Horn Y. & Tarascon J. M. Anionic redox processes for electrochemical devices. Nature Materials 15, 121–126, doi: 10.1038/nmat4551 (2016). [DOI] [PubMed] [Google Scholar]
  40. Sathiya M. et al. Reversible anionic redox chemistry in high-capacity layered-oxide electrodes. Nature Materials 12, 827–835, doi: 10.1038/Nmat3699 (2013). [DOI] [PubMed] [Google Scholar]
  41. Barker J., Koksbang R. & Saidi M. Y. An electrochemical investigation into the lithium insertion properties of LixNiO2 (0< = x < = 1). Solid State Ionics 89, 25–35, doi: 10.1016/0167-2738(96) 00262-7 (1996). [DOI] [Google Scholar]
  42. Perdew J. P. et al. Atoms, Molecules, Solids, and Surfaces - Applications of the Generalized Gradient Approximation for Exchange and Correlation. Phys Rev B 46, 6671–6687, doi: 10.1103/PhysRevB.46.6671 (1992). [DOI] [PubMed] [Google Scholar]
  43. Kresse G. & Furthmuller J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys Rev B 54, 11169–11186, doi: 10.1103/PhysRevB.54.11169 (1996). [DOI] [PubMed] [Google Scholar]
  44. Kresse G. & Furthmuller J. Efficiency of ab-initio total energy calculations for metals and semiconductors using a plane-wave basis set. Comp Mater Sci 6, 15–50, doi: 10.1016/0927-0256(96)00008-0 (1996). [DOI] [PubMed] [Google Scholar]
  45. Hubbard J. Electron Correlations in Narrow Energy Bands. Proc R Soc Lon Ser-A 276, 238, doi: 10.1098/rspa.1963.0204 (1963). [DOI] [Google Scholar]
  46. Lim J. M., Hwang T., Park M. S., Cho M. Cho K. Design of a p-type electrode for enhancing electronic conduction in high-Mn, Li-rich oxides. Chemistry of Materials 28, 8201–8209 doi: 10.1021/acs.chemmater.6b03032 (2016). [DOI] [Google Scholar]
  47. Lim J. M., Cho K., Cho M., Phase transformations with stress generations in electrochemical reactions of electrodes: Mechanics-based multiscale model for combined-phase reactions. Extreme Mechanics Letters, doi: 10.1016/j.eml.2016.10.008 (2016). [Google Scholar]
  48. Kim D., Lim J. M., Park M. S., Cho K. & Cho M. Phase Separation and d Electronic Orbitals on Cyclic Degradation in Li–Mn–O Compounds: First-Principles Multiscale Modeling and Experimental Observations. ACS Applied Materials & Interfaces doi: 10.1021/acsami.6b01595, doi: 10.1021/acsami.6b01595 (2016). [DOI] [PubMed] [Google Scholar]
  49. Cahn J. W. & Hilliard J. E. Free Energy of a Nonuniform System.1. Interfacial Free Energy. J Chem Phys 28, 258–267, doi: Doi 10.1063/1.1744102 (1958). [DOI] [Google Scholar]
  50. Zhou F., Maxisch T. & Ceder G. Configurational electronic entropy and the phase diagram of mixed-valence oxides: The case of LixFePO4. Phys Rev Lett 97, doi: ARTN 15570410.1103/PhysRevLett.97.155704 (2006). [DOI] [PubMed] [Google Scholar]
  51. Bray A. J. Theory of Phase-Ordering Kinetics. Adv Phys 43, 357–459, doi: 10.1080/00018739400101505 (1994). [DOI] [Google Scholar]
  52. Han B. C., Van der Ven A., Morgan D. & Ceder G. Electrochemical modeling of intercalation processes with phase field models. Electrochim Acta 49, 4691–4699, doi: 10.1016/j.electacta.2004.05.024 (2004). [DOI] [Google Scholar]
  53. Chen L. Q. & Shen J. Applications of semi-implicit Fourier-spectral method to phase field equations. Comput Phys Commun 108, 147–158, doi: 10.1016/S0010-4655(97)00115-X (1998). [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Supplementary Information
srep39669-s1.doc (45.5KB, doc)
Supplementary Video 1
Download video file (145.8KB, avi)
Supplementary Video 2
Download video file (330.6KB, avi)
Supplementary Video 3
Download video file (279.3KB, avi)
Supplementary Video 4
Download video file (347.7KB, avi)

Articles from Scientific Reports are provided here courtesy of Nature Publishing Group

RESOURCES