Abstract
Failure of hollow trees in urban areas is a worldwide concern, and it can be caused by different mechanisms, i.e. bending stresses or flattening-related failures. Here we derive a new analytical expression for predicting the bending moment for tangential cracking, and compare the breaking moment of various failure modes, including Brazier buckling, tangential cracking, shear failure and conventional bending failure, as a function of t/R ratio, where t and R are the trunk wall thickness and trunk radius, respectively, of a hollow tree. We use Taiwan red cypress as an example and show that its failure modes and the corresponding t/R ratios are: Brazier buckling (Mode I), tangential cracking followed by longitudinal splitting (Mode II) and conventional bending failure (Mode III) for 0 < t/R < 0.06, 0.06 < t/R < 0.27 and 0.27 < t/R < 1, respectively. The exact values of those ratios may vary within and among species, but the variation is much smaller than individual mechanical properties. Also, shear failure, another type of cracking due to maximum shear stress near the neutral axis of the tree trunk, is unlikely to occur since it requires much larger bending moments. Hence, we conclude that tangential cracking due to cross-sectional flattening, followed by longitudinal splitting, is dominant for hollow trunks. Our equations are applicable to analyse straight hollow tree trunks and plant stems, but are not applicable to those with side openings or those with only heart decay. Our findings provide insights for those managing trees in urban situations and those managing for conservation of hollow-dependent fauna in both urban and rural settings.
Keywords: bending failure, Brazier moment, tangential crack, hollow trunk, orthotropic material, Taiwan red cypress
1. Introduction
Hollow tubes have the advantages of resisting bending and torsional moments with a relatively lower weight per unit length than solid cylinders of the same weight [1]. Therefore, tubular structures have merits of a high strength-to-weight ratio and low weight per unit length, resulting in lower material costs. These hollow structures are ubiquitous in nature, such as bamboo stems, cereal stalks, decayed hollow tree trunks [2] and animal bones [3], as well as in artificial structures, such as buildings, bridge frames, athletic halls and aircraft fuselages. In assessing the hazards of old trees on roadsides and in parks, the hollowness is usually inspected by Resistograph®, a sensitive drilling-resistance measuring method and/or sonic tomography [4–6]. According to visual tree assessment (VTA) field observations by Mattheck et al. [7], a trunk wall thickness t to outer radius R ratio t/R of 0.3 is widely used as a criterion for diagnosing a risky tree. However, there is discrepancy between the VTA field observations and the critical trunk wall thickness for failure predicted by classic bending theory, which assumes that the cross section does not ovalize. More factors such as tangential cracking and orthotropic material properties must be taken into consideration. Understanding the mechanism is important from both safety and conservation perspectives. Natural tree hollows are valuable and often essential for many wildlife species. Hollow-bearing trees are being removed at a faster rate than hollows form in many parts of the world (urban and rural) [8]. There are ongoing declines in abundance of fauna dependent on hollow trees for survival. Many hollow trees are cut down from a fear that they may fall at some point in the future and injure someone. Yet many hollow trees are clearly structurally sound as they remain in place for decades. Our aim is to establish a theoretical framework for assessing safety that might result in retention of more hollow trees.
Tree trunks are subject to two kinds of loading, self-weight and wind load, either of which can result in mechanical damage or failure. Self-weight results from gravitational forces acting on the mass of tree, whereas wind load is the result of wind-induced drag forces acting on the crown and trunk. The axial compressive stress due to self-weight usually has a minor effect except for highly slanted trunks in which self-weight can induce large bending stresses due to the horizontal offset of the crown centroid from trunk base. By contrast, strong wind can significantly affect a tree's stability. Wind load acts on the tree crown and causes large bending moments on the trunk and root plate. These moments are the main sources of trunk failure and root overturning.
The breaking of thick-walled hollow tree trunks subjected to gale gusts at the crown usually results from bending stresses. Failure begins with fibre buckling on the compression side, followed by fibre tearing on the tension side. In this case, the shape of the cross section may remain almost unchanged until failure occurs, and classic bending theory can be used to calculate the bending strength of long, hollow trunks. But for thin-walled trunks, breaking can be due to cross-section flattening [7,9,10]. Figure 1 illustrates hollow-trunk failure of white ash (Fraxinus americana) due to cross-sectional flattening and flattening failure of bamboo (Bambusa oldhamii). When an elastic straight beam is subjected to a bending moment, it deforms and becomes a curve in the longitudinal direction. As a result of the deformation, strain on the convex side of the beam is extensive while that on the concave side is compressive. In this case, fibres on the convex side are under tensile stresses and those on the concave side are under compressive stresses; these stresses increase proportionally with the distance from the neutral axis which passes through the centroid of the cross section. Owing to the formation of a curve, transverse compressive forces occur on the convex and concave sides of a beam [11,12]. If the beam is hollow and thin-walled, these forces can ovalize the cross section and cause cracking before buckling. When ovalization occurs, both the moment of inertia and stiffness of the cross section decrease. Ultimately, the cross section collapses and buckles under a smaller moment than would occur due to pure bending stresses. As the cross section flattens, the curvature increases, and the bending moment reaches a maximum value, known as the Brazier moment [13,14]. Spatz & Niklas successfully used numerical simulations to predict the critical bending moments of various failure modes, including bending failure, tangential cracking failure due to ovalization, and Brazier buckling, as a function of the t/R ratio, slenderness and orthotropic material properties [2]. Although powerful, numerical simulations can sometimes come at the detriment of physical insight and predictive understanding of the interplay between key parameters. Here, we derive an analytical expression, using Castigliano's theorem [15], a strain energy method useful in the treatment of statically indeterminate problems, for predicting the bending moment at which the tangential cracking occurs, and provide a comprehensive comparison on the failure modes for 0 < t/R < 0.3. Direct calculation of the moments is convenient in assessing the stability of thin-walled hollow trunks, which is appealing from both safety and conservation perspectives.
2. Material and methods
2.1. Analysis of failure modes
In this section, we determine the failure mode at a given t/R ratio by comparing the magnitudes of the conventional bending moment (Mb), Brazier breaking moment (MB) and tangential cracking moment (Mc). The expressions for Mb and MB are obtained from the literature, and the expression for Mc derived in §2.1.3 is new and has not been reported before.
2.1.1. Failure by conventional bending (Mb)
Figure 2 illustrates a tree loaded with a wind load P at the centroid of its crown. The bending moment Mx at a distance h from the centroid is Ph. Assuming that the cross section of a tree trunk is circular, according to classical bending theory the maximum bending moment of a hollow tree trunk Mb is
2.1 |
where σb is the bending strength of typical green wood in the longitudinal direction. For small t/R, and for a solid trunk (t/R = 1), the bending moment is .
When bent, the side of tube furthest from the centre of curvature is in tension, and the other side is in compression. If the tensile stress exceeds the tensile strength of the wood material, the tube will fracture, resulting in a tearing failure. If, instead, the compressive stress exceeds the compressive strength, the tube will collapse, resulting in a local compression failure. Wood is a natural orthotropic material with fibres aligned along the tree axis, and its compressive strength is about one-third of the tensile strength. Accordingly, local compression failure is expected to occur at a slightly lower bending moment than the tearing failure.
2.1.2. Failure by Brazier buckling (MB)
When a long, straight cylinder is bent, its curvature is proportional to the bending moment. Tensile stresses on the convex side and compressive stresses on the concave side both produce transverse compressive forces which increase with the curvature. The Brazier moment describes the effect of ovalization on the buckling of thin tubes. Brazier noted that buckling can occur in a thin-walled tube subjected to bending moment because the cross section ovalizes. An initially circular tube becomes oval, decreasing its second area moment and stiffness, and collapses as a result of structural instability. If the cross section is assumed unchanged during bending, the bending moment is proportional to the curvature as predicted by classic bending theory. In reality ovalization of the cross section may occur if the t/R is small, and the relationship between the bending moment and curvature becomes nonlinear (figure 3). When considering cross-sectional flattening, there exists a maximum bending moment MB at which the tube becomes unstable and results in local kinking and collapse. This critical bending moment for isotropic materials is known as the Brazier buckling moment. Several authors [12,16–18] extend the Brazier moment for orthotropic materials as
2.2 |
where EL and ET are the longitudinal and tangential modulus of elasticity, respectively, νLT and νTL the Poisson's ratios. It is interesting to note that MB is directly obtained by replacing the Young's modulus E and Poisson's ratio ν with the geometric average and in Brazier's formula [13].
2.1.3. Failure by tangential cracking (Mc)
The bending deformation of the tube induces longitudinal tensile strain/stress on the convex side and compressive strain/stress on the concave side of tube. The tensile stress and compressive stress both produce inward forces towards the x-axis (neutral axis), which tend to ovalize the cross section [2,19] (figure 4a). The inward force dF per unit axial length and a circumferential width of R dθ set up by the bending stress σL induced by a bent tube with a radius of curvature ρ is (figure 4b)
2.3 |
Note that dF is a body force, not shear force, acting on the bulk of material. Substituting for ρ and σL into equation (2.3), we obtain
2.4 |
where I = πR3t is the moment of inertia of the circular cross section of a thin tube. Owing to symmetry only one quarter of the ring is considered. The total force per unit length F is expressed as
2.5 |
Equation (2.4) is then rearranged as dF = F sinθ dθ.
The magnitude of the tangential bending moment M0 per unit length acting on the axial cross section at φ = 0 is statically indeterminate and can be calculated using Castigliano's theorem. By using M(φ) as the moment of unit length at an angle φ from the x-axis (figure 4b) and Iz as the moment of inertia of unit length of the cross section, the strain energy U per unit length for one quarter of the section is
2.6 |
and the moment M(φ) is given by
2.7 |
A positive M(φ) tends to increase the local curvature at φ. Owing to the condition of symmetry the cross section at ϕ = 0 does not rotate during bending, such that
2.8 |
Because dM(ϕ)/dM0 = 1, we have
2.9 |
then
2.10 |
Substituting for M0 from equation (2.10) into equation (2.7), we obtain
2.11 |
and M(0) = M0 = FR/4; M(π/2) = −FR/4; M(π/4) = 0.
Using tangential bending strength σT the tangential bending moment at failure MT can be expressed as
2.12 |
Substituting for M(0) = MT = FR/4 and F from equation (2.5) into equation (2.12), we obtain longitudinal bending moment Mc at which the tangential cracking is initiated at φ = 0
2.13 |
Note that equation (2.13) is the most important result of this study; it is derived for the first time and has not been reported in the literature. The distribution of normal stresses in the axial section at φ = 0 can be obtained by superposing the stress (σ1) due to the normal force F and the stress (σ2) due to the bending moment M0 = FR/4. The ratio of these two components is , indicating that σ1 is negligible when .
Note that the maximum absolute value of M(φ) occurs at φ = 0 and π/2, and M(0) = −M(π/2) = FR/4. Hence when the applied bending moment Mx exceeds Mc, tangential cracking, followed by longitudinal splitting, may occur simultaneously at the four vertices of the oval ring, and the cracking occurs on the inner surfaces at φ = π/2 and 3π/2, and outer surfaces at φ = 0 and π.
2.1.4. Failure by longitudinal shear stress (Ms)
An alternative explanation for longitudinal cracking was suggested by Mattheck et al. [7], who emphasized that splitting can result from shear stresses in the axial direction. Consider a hollow cylindrical trunk as a cantilever loaded by a wind load P at its crown. The corresponding internal bending moment at a distance h from the centroid is Mx = Ph (figure 2), and the maximum shear stress τmax at the neutral axis is [19]
2.14 |
Substituting shear strength τs and Ms/h for τmax and P in equation (2.14), we obtain the breaking moment for shear
2.15 |
2.1.5. Critical t/R ratios
Critical ratios (t/R)cB, (t/R)Bb and (t/R)cb that determine the failure mode at a given t/R ratio are calculated by setting Mc = MB, MB = Mb and Mc = Mb, respectively, using , equations (2.2) and (2.13) as follows:
2.16 |
2.17 |
2.18 |
The equations derived in this section are applicable to analyse straight hollow trunks of tree species and bamboo stems, but are not applicable to those with side openings or those with only heart decay. Trunks with heart decay are more resistant to flattening failure; the theoretical analysis of hollow trunks with side openings is more complicated and is beyond the scope of this paper.
2.2. Experimental demonstration of tangential cracking
To experimentally illustrate the failure appearance of tangential cracking, we conducted computer-controlled compression tests (HT-9102, Hung Ta Instrument Co. Ltd.) on a hollow trunk of softwood (Araucaria cunninghamia). The hollow section, artificially created from a solid one with t = 30 mm and R = 125 mm (t/R = 0.24), was subjected to vertical point loads, and failed due to cross-sectional flattening (figure 5). We repeated the same experiment twice on A. cunninghamia and bamboo stems (B. oldhamii), and observed the same failure mode—cracking, followed by splitting---began on the outer surfaces of the left and right ends, and on the inner surfaces of the top and bottom positions, where the maximum tensile stresses are located. This failure appearance well corresponds to the tangential cracking predicted by our analysis in §2.1.3, and is consistent with earlier work by Mattheck [20] and Spatz & Niklas [2]. However, the loading here is external and is different from that which a tree really experiences during bending despite their similar failure appearance. The formula, based on external point loading [12], is expected to introduce some deviation from the actual case. On the other hand, equation (2.18) does not assume external point loading and is more accurate in predicting the critical t/R ratio.
3. Results and discussion
In this section, we describe our case studies of four tree species using the equations presented in §2. Their mechanical properties and critical t/R ratios are summarized in table 1. Figure 6a shows the failure moment ratios as a function of t/R for Taiwan red cypress (Chamaecyparis formosensis). Three dominant failure modes and their corresponding t/R ranges are determined as Brazier buckling (Mode I, 0 < t/R < 0.06), tangential cracking/longitudinal splitting (Mode II, 0.06 < t/R < 0.27) and conventional bending failure, i.e. compression failure on the compression side and tearing on the tension side (Mode III, 0.27 < t/R < 1). The critical ratios (t/R)cB, (t/R)Bb and (t/R)cb, calculated from equations (2.16–2.18), are 0.06, 0.13, and 0.27, respectively. Among them, Mode I and Mode II involve cross-sectional flattening and Mode III does not. Although a critical ratio of t/R = 0.13 exists for Brazier buckling, it is unlikely to occur since the breaking moment for tangential cracking Mc is much smaller.
Table 1.
Young's modulus (GPa) |
bending strength (MPa) |
||||||
---|---|---|---|---|---|---|---|
species | EL | ET | σb | σT | (t/R)cB | (t/R)Bb | (t/R)cb |
C. formosensisa | 4.9 | 0.25 | 45 | 2.2 | 0.06 | 0.13 | 0.27 |
A. cunninghamiaa | 9.9 | 0.50 | 71 | 3.5 | 0.05 | 0.10 | 0.21 |
T. boiviniib | 7.1 | 0.36 | 77 | 5.1 | 0.10 | 0.15 | 0.24 |
L. castanopsisifoliusb | 8.8 | 0.44 | 82 | 5.5 | 0.08 | 0.13 | 0.21 |
aSoftwood.
bHardwood.
The failure mode of the other three species, as a function of t/R ratio, is similar to that of Taiwan red cypress (table 1). Their (t/R)cb, the most important results of this work, range from 0.21 to 0.27. Our prediction of a tangential cracking at t/R < 0.27 is in remarkable agreement with the well-appreciated field observations conducted by Mattheck & Breloer [20]. They examined over 1000 broken and standing hardwood and softwood trees in parks and along roadsides, and found that most of the broken trees had t/R values < 0.3. Therefore, the ratio t/R = 0.3 has been used worldwide for VTAs as an approximate criterion for the upper critical limit in risk evaluation of decayed trunks. This excellent agreement indicates that our analysis captures the physics of the failure mechanism of trees.
Hollow tubes have the advantages of resisting bending and torsional moments with a relatively lower weight per unit length than solid cylinders of the same weight. A hollow trunk of t/R = 0.3 still contains a residual bending strength (Mb) of 76% of a solid one with the same outer radius (figure 6b). If we assume that a sound trunk has a safety factor of four [7], the safety factor of a hollow trunk with a t/R of 0.3 is three. However, the ratio drops significantly when t/R < 0.3, which is compounded by the cross-sectional flattening and makes those trees particularly vulnerable to bending.
Broken trees of t/R ratio below 0.05 are almost non-existent, suggesting that failure by Brazier buckling is indeed very rare in the field. Accordingly, tangential cracking followed by longitudinal splitting becomes the dominant failure mode of hollow trunks. Wegst & Ashby [12] also derived equations to calculate the bending moment for longitudinal splitting. They assumed external point loads similar to our experimental condition (figure 5). Those equations, although originally derived for plants with hollow stems, have been adopted to analyse mechanical failure in animal exoskeletons and endoskeletons [3]. We find that their formula for Mc at φ = 0 gives very similar results to equation (2.13) (less than 10% deviation for 0.1 < t/R < 1). However, due to the assumed external point loads, their formula predicts a much smaller Mc at φ = π/2 (approx. 73% of the Mc at φ = 0), meaning that the tangential cracking will always initiate at the load application points, i.e. φ = π/2 and 3π/2. By contrast, our analysis does not assume external point loads and predict that the tangential cracking initiates simultaneously at the four vertices of the oval ring. On the other hand, Spatz & Niklas [2] conducted comprehensive computer simulations to estimate the breaking moments for different failure modes. They assume that 10% ovalization leads to Brazier buckling, and critical failure strains are 0.3 and 2% in the axial and tangential directions, respectively. Their simulation results of (t/R)cB = 0.11 and (t/R)cb = 0.23 are remarkably close to those obtained by our formula, although different material properties are used (figure 6a). Besides, their simulation showed that cross-sectional flattening only plays a role for t/R < (t/R)cb, which is also consistent to our analysis.
An alternative explanation of longitudinal splitting is due to longitudinal shear stress, proposed by Mattheck et al. [7]. They reported that trunk failure begins with a shear crack combined with flattening of the cross section, followed by bending failure, and suggested that complex effects of shear, bending stress, longitudinal splitting and the Brazier moment should be considered in determining the mechanism of trunk breakage. Here we assume σb = 8.5 τs [22] and compare the magnitudes of bending moments, required to initiate shear failure and bending failure, by calculating Ms/Mb versus t/R and slenderness ratio h/R. Ms/Mb ratios increase with both t/R and h/R. Conventional bending failure is more dominant for trees with h/R > 10, whereas shear failure is only possible for extremely small h/R and thin-walled trunk (figure 6c). Spatz & Niklas [2] simulated the ratio of compressive stress to shear stress versus t/R and h/R, and also concluded that shear failure is unlikely to occur except for very short and thin-walled trunks. Nevertheless, by using finite-element method, Mattheck et al. [7] found that the ‘crossing’ of tensile and compressive stresses at the tree butt may significantly amplify the shear stress and initiate axial shear cracks even in solid trunks. This is an interesting viewpoint worth further research.
Growth stresses are ubiquitous in trees and may affect the failure mechanism. Longitudinal growth stress of normal wood is tensile on the surface of the trunk and is compressive inside [21,24,25], whereas tangential growth stresses are always compressive on the surface but tensile inside. Because the longitudinal compression strength of wood is only about one-third of its tensile strength, longitudinal tensile growth stresses can partially compensate for the compressive stresses on the leeward side of a trunk induced by the bending moment of wind loads acting on its crown. The compressive surface growth stress in the tangential direction can partially resist longitudinal splitting. These features may be recognized as the self-optimized design of trees as a result of evolution.
Hazard assessments of hollow trunks with respect to flattening failure can be achieved by comparing the Brazier moment, tangential splitting moment and bending failure moment with the wind load moment. To calculate the wind load moment, the wind speed of a hurricane (33 m s−1, Beaufort scale 12) is usually adopted as a standard. The crown area and centroid height can be estimated by image analysis. If the wind load moment is larger than these moments, it is possible that a hollow tree may fail.
4. Conclusion
In this paper, we investigate the failure mechanism of hollow trunks due to bending by comparing various failure modes, including Brazier buckling, tangential cracking/longitudinal splitting, conventional bending failure and shear failure. We derive a new analytical expression for predicting the bending moment at which tangential cracking occurs, and show that the cracking, followed by longitudinal splitting, is initiated simultaneously at the four vertices of the ovalized section. We use Taiwan red cypress as an example, and find that its dominant failure modes are Brazier buckling (Mode I), tangential cracking/longitudinal splitting (Mode II) and conventional bending failure (Mode III) for 0 < t/R < 0.06, 0.06 < t/R < 0.27 and 0.27 < t/R < 1, respectively. Among those, Mode I and Mode II are flattening-related failures. The critical value of (t/R)cb = 0.27 indicates that trees with a t/R < 0.27 tend to fail with longitudinal splitting, which is in remarkable agreement with the well-appreciated criterion of VTAs. Our analysis provides new insights into the understanding of hollow tree failures, in particular the origin of longitudinal splitting. Our findings may be readily applied to assess the failure potential of other tree species with different material properties. Our theoretical framework is applicable to analyse straight hollow tree trunks and plant stems, but is not applicable to those with side openings or those with only heart decay.
Supplementary Material
Data accessibility
The datasets for generating figure 6 have been uploaded as the electronic supplementary material alongside this article.
Authors' contributions
Y.-S.H. conceived and planned the study; F.-L.H. and C.-M.L. conducted the experiments and helped prepare the figures; Y.-S.H. and J.-Y.J. developed the theoretical derivations, discussed the results and wrote the manuscript. All authors gave final approval for publication.
Competing interests
We have no competing interests.
Funding
This study was partially supported by the Council of Agriculture, Taiwan through a research grant (102AS-13.2.7-FI-G8).
References
- 1.Galileo G. 1638. Discorsie dimonstrazioni matematichi, intorno a due nouvo scienze. Leida, Italy: Appresso gli Elsevirii. [Google Scholar]
- 2.Spatz H-C, Niklas KJ. 2013. Modes of failure in tubular plant organs. Am. J. Bot. 100, 332–336. (doi:10.3732/ajb.1200454) [DOI] [PubMed] [Google Scholar]
- 3.Taylor D, Dirks J-H. 2012. Shape optimization in exoskeletons and endoskeletons: a biomechanics analysis. J. R. Soc. Interface 9, 3480–3489. (doi:10.1098/rsif.2012.0567) [DOI] [PMC free article] [PubMed] [Google Scholar]
- 4.Larsson B, Bengtsson B, Gustafsson M. 2004. Nondestructive detection of decay in living trees. Tree Physiol. 24, 853–858. (doi:10.1093/treephys/24.7.853) [DOI] [PubMed] [Google Scholar]
- 5.Moore W. 1999. The combined use of the resistograph and the shigometer for the accurate mapping and diagnosis of the internal condition of woody support organs of trees. Arboric. J. 23, 273–287. (doi:10.1080/03071375.1999.9747245) [Google Scholar]
- 6.Lawday G, Hodges PA. 2000. The analytical use of stress waves for the detection of decay in standing trees. Forestry 73, 447–456. (doi:10.1093/forestry/73.5.447) [Google Scholar]
- 7.Mattheck C, Bethge K, Tesari I. 2006. Shear effects on failure of hollow trees. Trees Struct. Funct. 20, 329–333. (doi:10.1007/s00468-005-0044-0) [Google Scholar]
- 8.NSW Scientific Committee. 2011. Loss of Hollow-bearing trees—key threatening process determination. See http://www.environment.nsw.gov.au/determinations/lossofhollowtreesktp.htm.
- 9.Kane B, Ryan D, Bloniarz D. 2001. Comparing formulae that assess strength loss due to decay in trees. J. Arboric. 27, 78–87. [Google Scholar]
- 10.Bond J. 2006. Foundations of tree risk analysis: Use of the t/R ratio to evaluate trunk failure potential. Arborist News 15, 31–34. [Google Scholar]
- 11.Ennos AR, van Casteren A. 2010. Transverse stresses and modes of failure in tree branches and other beams. Proc. R. Soc. B 277, 1253–1258. (doi:10.1098/rspb.2009.2093) [DOI] [PMC free article] [PubMed] [Google Scholar]
- 12.Wegst UGK, Ashby MF. 2007. The structural efficiency of orthotropic stalks, stems and tubes. J. Mater. Sci. 42, 9005–9014. (doi:10.1007/s10853-007-1936-8) [Google Scholar]
- 13.Brazier LG. 1927. On the flexure of thin cylindrical shells and other thin sections. Proc. R. Soc. Lond. A 116, 104–114. (doi:10.1098/rspa.1927.0125) [Google Scholar]
- 14.Karam GN, Gibson LJ. 1995. Elastic buckling of cylindrical shells with elastic cores---I. Analysis. Int. J. Solids Struct. 32, 1259–1283. (doi:10.1016/0020-7683(94)00147-O) [Google Scholar]
- 15.Timoshenko S. 1955. Strength of materials. part I. Elementary theory and problems, 3rd edn New York, NY: Van Nostrand Reinhold. [Google Scholar]
- 16.Hayashi T. 1949. On the elastic instability of orthogonal anisotropic cylindrical shells, especially the buckling load due to compression, bending and torsion. J. Zosen Kiokai 1949, 85–98. (doi:10.2534/jjasnaoe1903.1949.85) [Google Scholar]
- 17.Baruch M, Arbocz J, Zhang GQ.1992. Imperfection sensitivity of the Brazier effect for orthotropic cylindrical shells. (http://repository.tudelft.nl/islandora/object/uuid:fd2ef265-fbe8-43ac-8200-a35200e6931e?collection=research. )
- 18.Takano A. 2013. Interaction between Euler buckling and Brazier instability. J. Solid Mech. Mater. Eng. 7, 92–101. (doi:10.1299/jmmp.7.92) [Google Scholar]
- 19.Timoshenko S, Young DH. 1962. Elements of strength of materials. New York, NY: Van Nostrand Reinhold. [Google Scholar]
- 20.Mattheck C, Breloer H. 1996. Body language of trees: a handbook for failure analysis. London, UK: Stationery Office Books. [Google Scholar]
- 21.Huang Y-S, Chen S-S, Kuo-Huang L-L, Lee C-M. 2005. Growth strain in the trunk and branches of Chamaecyparis formosensis and its influence on tree form. Tree Physiol. 25, 1119–1126. (doi:10.1093/treephys/25.9.1119) [DOI] [PubMed] [Google Scholar]
- 22.1999. Wood handbook—wood as an engineering material. Centennial edition Madison, WI: Forest Products Laboratory, Forest Service, United States Department of Agriculture. [Google Scholar]
- 23.Bodig J, Jayne BA. 1982. Mechanics of wood and wood composites. New York, NY: Van Nostrand Reinhold. [Google Scholar]
- 24.Archer RR. 1987. Growth stresses and strains in trees. New York, NY: Springer. [Google Scholar]
- 25.Dietrich F, Mattheck C. 1995. Cracks in sabre-shaped trees and branches. J. Theor. Biol. 173, 321–327. (doi:10.1016/s0022-5193(95)90001-2) [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Supplementary Materials
Data Availability Statement