Skip to main content
NIHPA Author Manuscripts logoLink to NIHPA Author Manuscripts
. Author manuscript; available in PMC: 2017 Oct 13.
Published in final edited form as: Adv Funct Mater. 2016 May 23;26(29):5345–5351. doi: 10.1002/adfm.201600713

Design of Strain-Limiting Substrate Materials for Stretchable and Flexible Electronics

Yinji Ma 1, Kyung-In Jang 2, Liang Wang 3, Han Na Jung 4, Jean Won Kwak 5, Yeguang Xue 6, Hang Chen 7, Yiyuan Yang 8, Dawei Shi 9, Xue Feng Prof 10, John A Rogers Prof 11,, Yonggang Huang Prof 12,
PMCID: PMC5639729  NIHMSID: NIHMS868068  PMID: 29033714

Abstract

Recently developed classes of electronics for biomedical applications exploit substrates that offer low elastic modulus and high stretchability, to allow intimate, mechanically biocompatible integration with soft biological tissues. A challenge is that such substrates do not generally offer protection of the electronics from high peak strains that can occur upon large-scale deformation, thereby creating a potential for device failure. The results presented here establish a simple route to compliant substrates with strain-limiting mechanics based on approaches that complement those of recently described alternatives. Here, a thin film or mesh of a high modulus material transferred onto a prestrained compliant substrate transforms into wrinkled geometry upon release of the prestrain. The structure formed by this process offers a low elastic modulus at small strain due to the small effective stiffness of the wrinkled film or mesh; it has a high tangent modulus (e.g., >1000 times the elastic modulus) at large strain, as the wrinkles disappear and the film/mesh returns to a flat geometry. This bilinear stress–strain behavior has an extremely sharp transition point, defined by the magnitude of the prestrain. A theoretical model yields analytical expressions for the elastic and tangent moduli and the transition strain of the bilinear stress–strain relation, with quantitative correspondence to finite element analysis and experiments.

1. Introduction

Significant progress in materials science, mechanical designs, and manufacturing approaches in stretchable and flexible electronics[14] has led to a broad range of recent system-level device demonstrators,[511] with emerging commercial examples in biomedical devices and wearable electronics.[1214] The soft mechanical behaviors of these systems represent key points of uniqueness relative to conventional technologies, where the requirements include: (i) low effective modulus and ability to accommodate large strain deformations with elastic response, to minimize mechanical constraints on biological tissues;[15] and (ii) small strains in the active materials to eliminate the possibility of device failure.[1618] One solution to the latter challenge involves development of active materials that themselves have high fracture strains.[1924] Alternatives rely on mechanics design in the substrate and in geometrically shaped material structures to maintain compatibility with the highest performance electronic materials, such as inorganic semiconductors. Here, materials (e.g., network materials,[25] network collagen fibrils,[26] biological tissue[27]) that have the “J-shaped” stress–strain behavior can be important. In some designs toward this goal,[25] curved microstructures in network layouts yield mechanics that involves compliant (low elastic modulus) response at small strain due to bending and twisting deformations. An effective stiffening occurs at large strain (high tangent modulus) as the microstructures straightened and transition from a bending to a stretching dominated response. The resulting materials properties satisfy the requirements outlined in the previous paragraph, although the ratio of the high tangent modulus to low elastic modulus can reach values of only ≈10. In addition, the transition between these two regimes occurs over a wide range of strains, instead of a more desirable sharp, bilinear response.

This paper introduces a simple strategy that overcomes these limitations. We begin with a description of a basic embodiment, consisting of a thin film of a stiff material bonded to a prestrained, compliant substrate (Figure 1). Release of the prestrain leads to wrinkling of the thin film into sinusoidal form.[28] At small strain, such a system has low elastic modulus, close to that of the compliant substrate, because the stiffness of the wrinkled film is negligible. Beyond an applied strain that stretches the wrinkled film into its original, flat geometry, the stiff film yields a high tangent modulus. The result is a bilinear stress–strain behavior with an extremely sharp transition point, and an exceptionally high ratio (e.g., >103) of tangent to elastic moduli. Comprehensive theoretical, numerical, and experimental studies of this composite material, and of advanced embodiments, reveal key variables that govern the strain-limiting behavior, under both uni- and multidirectional strain.

Figure 1.

Figure 1

Schematic illustrations and optical images of the process for fabricating strain-limiting structures. a,b) Compliant substrate without and with the prestrain. c) Transfer printing a stiff thin film onto the prestrained substrate. d) Releasing the prestrain to form the wrinkled film. e) Stretching the strain-limiting structure. f) Bilinear stress–strain behavior of the strain-limiting structure. g–i) Optical images (scale bar, 1 cm; inset scale bar: 0.5 mm) of the process for applying prestrain to the substrate, transfer printing a stiff thin film on the prestrained substrate, and releasing the prestrain to form the wrinkled film.

2. Results and Discussions

The schematic diagrams in Figure 1a–e illustrate the fabrication process. A compliant, elastomeric substrate with an initial length L1 and thickness H (Figure 1a) is stretched to length L2 (Figure 1b), to induce a prestrain εpre = (L2L1)/L1 in the substrate. A stiff thin film with thickness h is bonded onto the prestrained substrate (Figure 1c). Release of the prestrain in the substrate leads to wrinkling of the thin film (Figure 1d) to a length L0. This system of materials is then stretched to length L (Figure 1e), which defines the applied strain ε = (LL0)/L0. At small applied strain, the elastic modulus E of the system is the same as the elastic modulus ES of the compliant substrate, i.e., E = Es. This is because the membrane force in the wrinkled film remains constant during stretching such that the wrinkled film has a negligible stiffness and does not contribute to the tensile stiffness of the system. As the applied strain increases, the film begins to return to its flat state. At a strain comparable to the prestrain, the film becomes flat again and therefore contributes to the stiffness of system to yield the tangent modulus Etangent = (Efh + EsH)/(h + H) by the rule of mixtures,[29] where Ef is the elastic modulus of the film. As illustrated in Figure 1f, the behavior follows a bilinear stress–strain relation, with a transition strain εtransition = (L2L0)/L0 that separates the two linear regimes. For a thin film (e.g., h = ≈10−3H) much stiffer than the substrate (e.g., Ef = ≈106Es), the tangent modulus Etangent is much larger than the elastic modulus Es of the system, thereby providing a strain-limiting response. Figure 1g–i shows optical images for various stages in the fabrication, corresponding to Figure 1b–d, respectively, for the case of a polyimide (PI) thin film and a silicone (Silbione) substrate. PI has been widely used in stretchable electronics.[30,31] Their elastic properties appear in Table 1, together with those of Cu (as the stiff thin film), and polydimethylsiloxane (PDMS, Sylgard 184, 10:1 ratio of prepolymer and curing agent) and Ecoflex for the compliant substrate.

Table 1.

Maximum prestrain and material properties of representative systems.

PDMS [Es = 1 MPa, νs = 0.5] Ecoflex [Es = 60 kPa, νs = 0.5] Silbione [Es = 3 kPa, νs = 0.5]
Cu (Ef= 119 GPa, νf = 0.34, εY = 0.3%) 0.8% 6.0% 45%
PI (Ef= 2.5 GPa, νf= 0.34, εY = 2%) 2.6% 20% 150%

The total energy consists of the membrane energy and bending energy in the thin film, and the elastic strain energy in the compliant substrate. Minimization of the total energy gives the wrinkle wavelength and amplitude.[28,32] For a semi-infinite substrate, its initial length L1 is recovered upon release of the prestrain, i.e., L0 = L1 in Figure 1d, and the transition strain for the bilinear stress–strain relation is simply the prestrain, i.e., εtransition = εpre. This relation εtransition = εpre holds approximately for a very thick substrate when its bending stiffness overwhelms that of the film, i.e., Ēfh3/(ĒsH3) ≪ 0.01. The transition strain for a relatively thick substrate [Ēfh3/(Ēsh3) < ≈ 0.01] will be discussed in Equations (3) and (7). Here E¯s=Es/(1νs2) and E¯f=Ef/(1νf2) are the plane-strain moduli of the substrate and film, respectively, and νs and νf are the corresponding Poisson's ratios. The critical strain for wrinkling is εc = (3Ēs/Ēf)2/3/4, which is ≈0.3% or much less for the materials in Table 1. Once wrinkled, the compressive membrane strain in the film remains at −εc. The bending strain reaches a maximum upon complete release of the prestrain, and is given by 2ɛc(ɛpreɛc)2ɛcɛpre since the prestrain is usually much larger than εc. The maxi mum strain in the film, which is the same as the bending strain since the membrane strain is negligible, should be less than the yield strain εY of the film in order to avoid plastic deformation, which gives a maximum prestrain of

ɛpre<ɛY24ɛc=ɛY2(E¯f3E¯s)2/3 (1)

As shown in Table 1, the maximum prestrain for PI is much larger than that for Cu because PI has a relatively large yield strain εY = 2%.[25] The maximum prestrain for Silbione is much larger than those for Ecoflex and PDMS, which is consistent with Equation (1). This is because Silbione has very low elastic modulus and therefore imposes small stress on the film at the same prestrain.

Applications of strain-limiting materials may require relatively thin substrates.[33] For substrates with bending stiffness two (or more) order(s) of magnitude or above that of the film, i.e., Ēfh3/(ĒsH3) <≈0.01, numerical results for the substrate with finite thickness[34] suggest that the analysis described above is still valid. However, the substrate no longer recovers its initial length L1 upon release of the prestrain, due to the film stiffness. The residual force Ēfc in the substrate resulting from the membrane strain −εc in the film, gives the new length L0 of the substrate as (Figure 1d)

L0=L1+L14(9E¯fh3E¯sH3)1/3 (2)

This value increases with the ratio of film-to-substrate bending stiffness, as shown in Figure S1 in the Supporting Information of the normalized length L0/L1 versus thickness ratio H/h for the PI film on several substrates. The transition strain for the bilinear stress–strain relation is

ɛtransition=ɛpre14(9E¯fh3E¯sH3)1/31+14(9E¯fh3E¯sH3)1/3 (3)

It degenerates to εtransition = εpre for a semi-infinite substrate (H → ∞). This expression suggests that the prestrain must exceed [9Ēfh3/(Ēsh3)]1/34 for the system to exhibit a bilinear stress-strain relation. Besides the transition strain, the other critical property is the tangent modulus, and is obtained from the rule of mixtures[29] as

E¯tangent=E¯fh+E¯sHh+HE¯s+hHE¯f (4)

Figure 2a shows the bilinear stress–strain curves for a 1 μm-thick PI film on a 1 mm-thick Silbione substrate. The results from finite element analysis (FEA) and experiments agree well with the theory. The prestrain εpre is 15.1%, 25.6%, and 36.0% for the transition strain εtransition to be 10%, 20%, and 30%, respectively. Here the prestrain must be larger than the transition due to the finite thickness of the substrate. Figure 2b shows the linear relation between εtransition and εpre in Equation (3) for the PI film on several substrates given in Table 1 with the substrate-to-film thickness ratio H/h = 1000. The intercept of each curve with the horizontal axis denotes the minimal prestrain for wrinkling obtained from Equation (3), below which the film remains straight (but stretched) upon release of the prestrain. The right end of each curve denotes the maximum prestrain, determined from Equation (1) to avoid plastic yielding, but with εpre replaced by εtransition to account for the finite thickness of the substrate (see Note 1 in Supporting Information for details). A more compliant substrate gives a larger range of prestrain that avoids plastic yielding, but also requires a larger prestrain to trigger wrinkling. The maximum prestrain can reach 150% for PI/Silbione. Figure 2c shows the linear relation between the tangent modulus Ētangent and film stiffness Ēfh in Equation (4) for the PI film on several substrates with thickness ratios H/h = 1000, 3000, and 5000. A thinner substrate clearly gives a higher tangent modulus, reaching >1000 times of the elastic modulus as shown in Figure 2c.

Figure 2.

Figure 2

Theoretical, numerical, and experimental results from a unidirectional strain–limiting structure. a) Bilinear stress–strain curves of 1 μm-thick PI film on 1 mm-thick Silbione substrate subjected to various prestrains. b) The transition strain versus the prestrain for the PI film on several substrates with thickness ratio H/h = 1000. c) The tangent modulus normalized by the substrate modulus, Ētangent/Ēs, versus the normalized film modulus Ēf/Ēs for several thickness ratios H/h. d) The critical film length that separates local wrinkling from global buckling. e,f) Numerical results and optical images (scale bar, 1 mm) of the morphology and out-of-plane displacement for a 1 μm-thick PI film on a 1 mm-thick Silbione substrate subjected to 15.1% prestrain.

There exists, however, a lower limit of the substrate thickness, below which global buckling occurs (top inset, Figure 2d), similar to Euler buckling of beams.[35] This lower limit is given by Ēfh3/(ĒsH3) = 0.064 (see Note 2 in Supporting Information for details). For the substrate thickness above this lower limit, global buckling may still occur if the initial length L1 is above a critical length Lcr[35] (see Note 2 in Supporting Information for details)

Lcr=8.7EIE¯sH[1(E¯sE¯f)2/3+(E¯fh3E¯sH3)1/310.0641/3] (5)

where

EI=(E¯sH2+E¯fh2)2+4E¯sE¯fH3h12(E¯sH+E¯fh) (6)

is the effective bending rigidity. The normalized critical length Lcr/h, which separates local wrinkling from the undesirable global buckling modes, is shown versus the substrate-to-film thickness ratio H/h for PI film on several substrates. For PI/Silbione and H/h = 1000, the length of the stiff thin film (L1) should be less than 15 000 times the thickness h. Figure 2e,f shows the morphology and out-of-plane displacement of 1 μm PI film on 1 mm Silbione, obtained by FEA and experiment, respectively, at 15.1% prestrain, which corresponds to 10% transition strain. The morphologies for 25.6% and 36.0% prestrain, corresponding to 20% and 30% transition strain, respectively, appear in Figure S2 in the Supporting Information.

Figure 3a shows a strain-limiting design for biaxial stretching. Here, the thin film in Figure 1c is replaced by a thin mesh (width W and spacing S, Figure 3a) on a biaxially pre-strained, compliant substrate. The thin mesh wrinkles in both x and y directions (Figure 3a) upon release of biaxial prestrains ɛprex and ɛprey. Such a design can achieve anisotropic strain-limiting behavior by applying different prestrains in x and y directions. Figure 3b shows the stress–strain curves for x-, y-and 45°-stretching of a 1 μm-thick PI mesh (width W = 0.1 mm and spacing S = 0.4 mm) on a 1 mm-thick Silbione substrate subjected to the prestrains ɛprex=30.8% and ɛprey=15.7%. For stretching along x or y directions, the stress–strain curves are clearly bilinear, and have the same elastic modulus Ēs, same tangent modulus given by ĒtangentĒs+ [W/(W + S)]Efh/H but different transition strains given by

Figure 3.

Figure 3

a) Schematic illustrations of the fabrication process that uses biaxial stretching. b) Stress-–strain curves for x-, y-, and 45°-stretching of 1 μm-thick PI mesh (width W = 0.1 mm and spacing S = 0.4 mm) on 1 mm-thick Silbione substrate subjected to prestrains of ɛprex=30.8% and ɛprey=15.7%. c) The transition strain versus the prestrain for the PI mesh on several substrates with thickness ratio H/h = 1000 and W/S = 1/4. d) The tangent modulus normalized by the substrate modulus, Ētangent/Ēs, versus (W/(W + S)) for PI mesh on several substrates with thickness ratio H/h = 1000. e,f) Numerical results and optical images (scale bar, 200 μm) of morphology and out-of-plane displacement for 1 μm-thick PI mesh (width W = 0.1 mm and spacing S = 0.4 mm) on 1 mm-thick Silbione substrate subjected to prestrains of ɛprex=30.8% and ɛprey=15.7%.

ɛtransitioni=ɛpreiW6(W+s)(9E¯fh3E¯sH3)1/31+W6(W+s)(9E¯fh3E¯sH3)1/3 (7)

where the superscript i denotes either x or y. The transition strain in the x or y direction depends only on the prestrain in the same direction, and is 30% for ɛprex=30.8% and 15% for ɛprey=15.7%, respectively in Figure 3b. The transition strain is comparable to the prestrain because the minimal prestrain [W/(W + S)][9Efh3(Ēsh3)]1/3/6 to initiate wrinkling is much smaller than that for uniaxial stretching due to the factor W/(W + S). For x- or y- stretching, the theory agrees well with FEA and experiments (Figure 3b). For stretching along 45° (Figure 3b) and other directions (Figure S3, Supporting Information), FEA and experiments all show the strain-limiting behavior, though they do not display a sharp transition point. Figure 3c shows the linear relation between ɛtransitioni and ɛprei in Equation (7) for the PI film on several substrates with the thickness ratio H/h = 1000 and width-to-spacing ratio W/S = 1/4. The minimal prestrain for wrinkling, corresponding to the intercept of each curve with the horizontal axis, is relatively small such that ɛtransitioniɛprei. The right end of each curve denotes the maximum prestrain for plastic yielding, and it increases as the substrate modulus decreases. Figure 3 d shows the linear relation between the tangent modulus Ētangent and [W/(W + S)]Ēfh/H for the PI film on several substrates with the thickness ratio H/h = 1000. The right limit W/(W + S) = 1 in Figure 3d (i.e., spacing S approaching 0) corresponds to Figure 2c for the thin film, while the limit W/(W + S) = 0 (i.e., no mesh) gives the substrate modulus. Figure 3e,f shows the morphology and out-of-plane displacement of a 1 μm PI mesh (width W = 0.1 mm, spacing S = 0.4 mm) on a 1 mm Silbione substrate, obtained by FEA and experiment, respectively, at the prestrains ɛprex=30.8% and ɛprey=15.7%. The results agree reasonably well, even though the optical image in Figure 3f shows slight delamination between the stiff thin mesh and compliant substrate. FEA (Figure S4, Supporting Information) also confirms that the effect of delamination, if any, is small (see Note 3 in the Supporting Information for details).

3. Conclusions

A thin film or mesh of a stiff material bonded onto a prestrained, compliant substrate wrinkles upon release of the prestrain. The resulting system is naturally strain-limiting—it has low elastic modulus, comparable to that of the substrate, at small strain because the wrinkled film or mesh has negligible stiffness in this regime; it has high tangent modulus (e.g., >1000 times the elastic modulus) at large strain when the wrinkled stiff film or mesh becomes flat. The result is a bilinear stress–strain response with a very sharp transition point. A theoretical model provide analytical expressions for the elastic and tangent moduli and the transition strain of the bilinear stress–strain relation, all in agreement with FEA and experiments.

For biomedical device applications, the low elastic modulus response can match or reach values below those of targeted biological tissues, thereby avoiding any mechanical constraint on natural motions. The high tangent modulus, on the other hand, serves to shield the stretchable and flexible electronics from large deformations that might otherwise lead to fracture and device failure.

4. Experimental Section

Finite Element Analysis

ABAQUS commercial software[36] was used to study the mechanics response of the strain-limiting structure. The compliant substrates (PDMS, Ecoflex and Silbione) were modeled by the hexahedron element (C3D8R), while the stiff thin films (Cu and PI) were modeled by the composite shell element (S4R).

Preparation of Strain-Limiting Structure

PMMA (100 nm) coated on a glass slide (70 × 50 × 1.0 mm3) served as a sacrificial layer to facilitate release. Spin casting on top of this substrate yielded a film of PI (1≈100 μm in thickness, HD Microsystems, USA). Photolithographic patterning of this PI followed by thermal curing (2 h at 250 °C in a vacuum oven) defined the desired planar or mesh structure. Undercut etching removed the PMMA layer to allow release for subsequent integration with a prestrained compliant and tacky elastomeric substrate (Silbione RT 4717 A/B, Bluestar silicones, France) mounted on a manual stretcher.

Measurements of Stress–Strain Responses

Mechanical properties of all samples were measured with a dynamic mechanical analyzer (TA instruments, Q800). Characterizing the applied force versus the displacement under uniaxial tensile loading at room temperature yielded data for determination of the mechanical modulus. Each of the reported results corresponds to an average of measurements on three samples.

Supplementary Material

SI

Acknowledgments

Y.M. and K.-I.J. contributed equally to this work. Y.M. and X.F. acknowledge the support from the National Basic Research Program of China (Grant No. 2015CB351900) and National Natural Science Foundation of China (Grant Nos. 11402135 and 11320101001). Y.H. acknowledges the support from NSF (DMR-1121262, CMMI-1300846, and CMMI-1400169) and the NIH (Grant No. R01EB019337).

Footnotes

Supporting Information: Supporting Information is available from the Wiley Online Library or from the author.

Contributor Information

Yinji Ma, Departments of Civil and Environmental Engineering, Mechanical Engineering, and Materials Science and Engineering, Northwestern University, Evanston, IL 60208, USA; Department of Engineering Mechanics, Center for Mechanics and Materials, Tsinghua University, Beijing 100084, China

Kyung-In Jang, Department of Materials Science and Engineering and Frederick Seitz Materials Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA

Liang Wang, Departments of Civil and Environmental Engineering, Mechanical Engineering, and Materials Science and Engineering, Northwestern University, Evanston, IL 60208, USA; Institute of Chemical Machinery and Process Equipment, Department of Chemical and Biological Engineering, Zhejiang University, Hangzhou 310027, China.

Han Na Jung, Department of Materials Science and Engineering, and Frederick Seitz Materials Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA.

Jean Won Kwak, Department of Materials Science and Engineering, and Frederick Seitz Materials Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA.

Yeguang Xue, Departments of Civil and Environmental Engineering, Mechanical Engineering, and Materials Science and Engineering, Northwestern University, Evanston, IL 60208, USA.

Hang Chen, Departments of Civil and Environmental Engineering, Mechanical Engineering, and Materials Science and Engineering, Northwestern University, Evanston, IL 60208, USA; Department of Engineering Mechanics, Center for Mechanics and Materials, Tsinghua University, Beijing 100084, China

Yiyuan Yang, Department of Materials Science and Engineering, and Frederick Seitz Materials Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA.

Dawei Shi, Department of Materials Science and Engineering, and Frederick Seitz Materials Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA.

Xue Feng, Prof., Department of Engineering Mechanics, Center for Mechanics and Materials, Tsinghua University, Beijing 100084, China

John A. Rogers, Prof., Departments of Materials Science and Engineering, Chemistry, Mechanical Science and Engineering, Electrical and Computer Engineering, Beckman Institute for Advanced Science and Technology and Frederick Seitz Materials, Research Laboratory, University of Illinois at Urbana-Champaign, Urbana, IL 61801, USA

Yonggang Huang, Prof., Departments of Civil and Environmental Engineering, Mechanical Engineering, and Materials Science and Engineering, Northwestern University, Evanston, IL 60208, USA

References

  • 1.Lu NS, Yang SX. Curr Opin Solid St M. 2015;19:149. [Google Scholar]
  • 2.Su YW, Wang SD, Huang YA, Luan HW, Dong W, Fan JA, Yang QL, Rogers JA, Huang Y. Small. 2015;3:367. doi: 10.1002/smll.201401181. [DOI] [PubMed] [Google Scholar]
  • 3.Kim DH, Lu NS, Huang YG, Rogers JA. MRS Bull. 2012;37:226. [Google Scholar]
  • 4.Wang C, Hwang D, Yu ZB, Takei K, Park J, Chen T, Ma BW, Javey A. Nat Mater. 2013;12:899. doi: 10.1038/nmat3711. [DOI] [PubMed] [Google Scholar]
  • 5.Webb RC, Ma J, Krishnan S, Li Y, Yoon S, Guo X, Feng X, Shi Y, Seidel SM, Cho NH, Kurniawan J, Ahad J, Sheth N, Kim J, Taylor JG, VI, Darlington T, Chang K, Huang W, Ayers J, Gruebele A, Pielak RM, Slepian MJ, Huang Y, Gorbach AM, Rogers JA. Sci Adv. 2015;1:e1500701. doi: 10.1126/sciadv.1500701. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 6.Hussain AM, Ghaffar FA, Park SI, Rogers JA, Shamim A, Hussain MM. Adv Funct Mater. 2015;25:6565. [Google Scholar]
  • 7.Liao CZ, Zhang M, Yao MY, Hua T, Li L, Yan F. Adv Mater. 2015;27:7493. doi: 10.1002/adma.201402625. [DOI] [PubMed] [Google Scholar]
  • 8.Zeng W, Shu L, Li Q, Chen S, Wang F, Tao XM. Adv Mater. 2014;26:5310. doi: 10.1002/adma.201400633. [DOI] [PubMed] [Google Scholar]
  • 9.Chen Y, Lu BW, Chen YH, Feng X. Sci Rep. 2015;5:11505. doi: 10.1038/srep11505. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 10.Stoppa M, Chiolerio A. Sensors. 2014;14:11957. doi: 10.3390/s140711957. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 11.Lu BW, Chen Y, Ou DP, Chen H, Diao LW, Zhang W, Zheng J, Ma WG, Sun LZ, Feng X. Sci Rep. 2015;5:16065. doi: 10.1038/srep16065. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 12.MC10, Inc. [accessed: January 2016]; http://mc10inc.com.
  • 13.BBC. L'Oreal unveils super-thin smart skin patch. [accessed: January 2016]; http://www.bbc.com/news/technology-35238636.
  • 14.NCC. Electronic skin makes your body a computer. [accessed: January 2016]; http://www.cnn.com/2015/05/15/tech/electronic-skin/
  • 15.Lee CH, Ma YJ, Jang KI, Banks A, Pan T, Feng X, Kim JS, Kang D, Raj MS, McGrane BL, Morey B, Wang XY, Ghaffari R, Huang YG, Rogers JA. Adv Funct Mater. 2015;25:3698. [Google Scholar]
  • 16.Park SI, Ahn JH, Feng X, Wang SD, Huang YG, Rogers JA. Adv Funct Mater. 2008;18:2673. [Google Scholar]
  • 17.Zhang YH, Wang SD, Li XT, Fan JA, Xu S, Song YM, Choi KJ, Yeo WH, Lee W, Nazaar SN, Lu BW, Yin L, Hwang KC, Rogers JA, Huang YG. Adv Funct Mater. 2014;24:2028. [Google Scholar]
  • 18.Chen H, Lu BW, Lin Y, Feng X. IEEE Electr Device L. 2014;35:132. [Google Scholar]
  • 19.Sekitani T, Noguchi Y, Hata K, Fukushima T, Aida T, Someya T. Science. 2008;321:1468. doi: 10.1126/science.1160309. [DOI] [PubMed] [Google Scholar]
  • 20.Sekitani T, Nakajima H, Maeda H, Fukushima T, Aida T, Hata K, Someya T. Nat Mater. 2009;8:494. doi: 10.1038/nmat2459. [DOI] [PubMed] [Google Scholar]
  • 21.McAlpine MC, Ahmad H, Wang DW, Heath JR. Nat Mater. 2007;6:379. doi: 10.1038/nmat1891. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 22.Liu ZF, Fang S, Moura FA, Ding JN, Jiang N, Di J, Zhang M, Lepro X, Galvao DS, Haines CS, Yuan NY, Yin SG, Lee DW, Wang R, Wang HY, Lv W, Dong C, Zhang RC, Chen MJ, Yin Q, Chong YT, Zhang R, Wang X, Lima MD, Ovalle-Robles R, Qian D, Lu H, Baughman RH. Science. 2015;349:400. doi: 10.1126/science.aaa7952. [DOI] [PubMed] [Google Scholar]
  • 23.Gaj MP, Wei A, Fuentes-Hernandez C, Zhang YD, Reit R, Voit W, Marder SR, Kippelen B. Org Electr. 2015;25:151. [Google Scholar]
  • 24.Xu F, Zhu Y. Adv Mater. 2012;24:5117. doi: 10.1002/adma.201201886. [DOI] [PubMed] [Google Scholar]
  • 25.Jang KI, Chung HU, Xu S, Lee CH, Luan HW, Jeong J, Cheng HY, Kim GT, Han SY, Lee JW, Kim J, Cho M, Miao FX, Yang YY, Jung HN, Flavin M, Liu H, Kong GW, Yu KJ, Rhee SI, Chung J, Kim B, Kwak JW, Yun MH, Kim JY, Song YM, Paik U, Zhang YH, Huang Y, Rogers JA. Nat Commun. 2015;6:11. doi: 10.1038/ncomms7566. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 26.Meyers MA, McKittrick J, Chen PY. Science. 2013;339:773. doi: 10.1126/science.1220854. [DOI] [PubMed] [Google Scholar]
  • 27.Provenzano PP, Heisey D, Hayashi K, Lakes R, Vanderby R. J Appl Physiol. 2002;92:362. doi: 10.1152/jappl.2002.92.1.362. [DOI] [PubMed] [Google Scholar]
  • 28.Khang DY, Jiang HQ, Huang Y, Rogers JA. Science. 2006;311:208. doi: 10.1126/science.1121401. [DOI] [PubMed] [Google Scholar]
  • 29.Daniel IM, Ishai O. Engineering Mechanics of Composite Materials. Oxford University Press; New York, USA: 2013. [Google Scholar]
  • 30.Kaltenbrunner M, Sekitani T, Reeder J, Yokota T, Kuribara K, Tokuhara T, Drack M, Schwodiauer R, Graz I, Bauer-Gogonea S, Bauer S, Someya T. Nature. 2013;499:458. doi: 10.1038/nature12314. [DOI] [PubMed] [Google Scholar]
  • 31.Fukuda K, Sekitani T, Someya T. Appl Phys Lett. 2009;95:023302. [Google Scholar]
  • 32.Jiang HQ, Khang DY, Song JZ, Sun YG, Huang YG, Rogers JA. Proc Natl Acad Sci USA. 2007;104:15607. doi: 10.1073/pnas.0702927104. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 33.Xu LZ, Gutbrod SR, Ma YJ, Petrossians A, Liu YH, Webb RC, Fan JA, Yang ZJ, Xu RX, Whalen JJ, Weiland JD, Huang YG, Efimov IR, Rogers JA. Adv Mater. 2015;27:1731. doi: 10.1002/adma.201405017. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 34.Huang ZY, Hong W, Suo Z. J Mech Phys Solids. 2005;53:2101. [Google Scholar]
  • 35.Wang SD, Song JZ, Kim DH, Huang YG, Rogers JA. Appl Phys Lett. 2008;93:3. [Google Scholar]
  • 36.ABAQUS. Analysis User's Manual. 2010 V6.10. [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

SI

RESOURCES