Table 1.

Theoretical and experimental density and a crystallinity degree of PCM.

Content of CF, wt % Theoretical Density, g/cm3 Experimental Density, g/cm3 XRD, %
PTFE/CF PTFE/CF/Kl PTFE/CF/Vl PTFE/CF PTFE/CF PTFE/CF/Kl PTFE/CF/Vl
0 2.20 2.15 ± 0.01 2.16 ± 0.01 2.16 ± 0.01 63 ± 1 65 ± 1 64 ± 1
1 2.19 2.15 ± 0.01 2.16 ± 0.01 2.15 ± 0.01 64 ± 1 67 ± 1 66 ± 1
3 2.18 2.13 ± 0.01 2.14 ± 0.01 2.13 ± 0.01 68 ± 1 69 ± 1 69 ± 1
5 2.16 2.11 ± 0.01 2.11 ± 0.01 2.10 ± 0.01 69 ± 1 72 ± 1 71 ± 1
8 2.13 2.09 ± 0.01 2.08 ± 0.01 2.06 ± 0.01 71 ± 1 74 ± 1 73 ± 1
10 2.11 2.06 ± 0.01 2.06 ± 0.01 2.03 ± 0.01 73 ± 1 74 ± 1 74 ± 1

Note: CF—carbon fiber; Kl—kaolinite; Vl—vermiculite; Vl and Kl contents are 1 wt %.