Abhay Shivayogimath 1,2, Joachim Dahl Thomsen 1,2, David M A Mackenzie 2,3, Mathias Geisler 2,4, Raluca-Maria Stan 5, Ann Julie Holt 5, Marco Bianchi 5, Andrea Crovetto 6, Patrick R Whelan 1,2, Alexandra Carvalho 7, Antonio H Castro Neto 7, Philip Hofmann 5, Nicolas Stenger 2,4, Peter Bøggild 1,2, Timothy J Booth 1,2,
PMCID: PMC6609655  PMID: 31273207

Abstract

Only a few of the vast range of potential two-dimensional materials (2D) have been isolated or synthesised to date. Typically, 2D materials are discovered by mechanically exfoliating naturally occurring bulk crystals to produce atomically thin layers, after which a material-specific vapour synthesis method must be developed to grow interesting candidates in a scalable manner. Here we show a general approach for synthesising thin layers of two-dimensional binary compounds. We apply the method to obtain high quality, epitaxial MoS2 films, and extend the principle to the synthesis of a wide range of other materials—both well-known and never-before isolated—including transition metal sulphides, selenides, tellurides, and nitrides. This approach greatly simplifies the synthesis of currently known materials, and provides a general framework for synthesising both predicted and unexpected new 2D compounds.

Subject terms: Synthesis and processing, Two-dimensional materials


The scalable synthesis of 2D materials critically relies on finding appropriate vapour-phase metal precursors and careful fine-tuning of growth parameters. Here, the authors instead use solid elemental precursors and a single recipe to demonstrate a general approach for synthesising thin epitaxial layers of 20 different 2D binary compounds, including transition metal sulphides, selenides, tellurides, and nitrides.

Introduction

Many of the possible 2D materials are binary compounds of the form MXn, where M is typically a transition metal and X a chalcogen or non-metal from groups IV, V, or VI15. The molybdenum and tungsten disulphides and diselenides remain the most commonly studied 2D binary compounds—other than hexagonal boron nitride (hBN)—due to the ready availability of naturally occurring bulk crystals amenable to exfoliation. Chemical vapour deposition (CVD) techniques for the scalable synthesis of these materials are available6; however, controlling the stoichiometry and hence the defect density can be challenging. Such techniques typically employ solid metal oxide710 or metal-organic11 precursors which are chalcogenated at elevated temperatures. Finding appropriate metal precursors can be a limiting challenge for extending these methods to other 2D transition metal compounds, and as a result requires single-process dedicated equipment that is highly optimised for growing one specific material. A more general method using simpler precursors would thus be beneficial. Published CVD growth models for binary compounds on metal catalysts stipulate that both M and X elements be insoluble in the catalyst to ensure surface-limited growth1214, by analogy with CVD graphene growth on copper15. In fact, the synthesis of monolayer hBN films on copper—despite the high solubility of boron in copper16—suggests that only one component need be insoluble.

Here we present a general method for synthesising two-dimensional compounds on a metal catalyst from solid elemental precursors (Fig. 1). We arrange a single component solid solution, as used for hBN growth on copper, by alloying metal M films with gold, which has limited solubility of the X elements (X = S, Se, Te, N). In brief, a thin layer (~20 nm) of metal M is sputtered onto a c-plane sapphire substrate followed by a thick layer (~ 500 nm) of gold (see Methods). The M-Au layer is then heated to 850 °C to form an alloy with an Au {111} surface. The relative thicknesses of the M and Au layers determines the concentration of M in the final alloy, which here is deliberately limited to ≤5 at%1724 in order to maintain single-phase alloying conditions. The Au-M alloy is subsequently exposed to a vapour-phase precursor of element X. The limited solubility of X in the gold restricts the formation of MXn compounds to the surface of the alloy—at the solid–gas interface—resulting in few-atom thick layers of binary compounds that are epitaxially aligned to the underlying Au substrate.

Fig. 1.

Fig. 1

Schematic overview of the synthesis process. A thin layer (~20 nm) of metal M is sputtered onto a c-plane sapphire substrate, and a thick layer (~500 nm) of Au is sputtered on top. The sample is annealed at 850 °C to produce an Au-M alloy, which is then exposed to a vapour of S, Se, Te, or more generally an elemental X gas or vapour. The growth of binary MXn compounds proceeds at the surface of the Au-M layer and is surface-limited

The process enables the epitaxial synthesis of both known and new 2D materials using a single recipe and simple elemental precursors, demonstrated here by the synthesis of 20 compounds including sulphides, selenides, tellurides, and nitrides.

Results

Synthesis and characterisation of MoS2

To benchmark this approach we first synthesise and characterise MoS2 layers (Fig. 2). Individual domains display triangular morphology as seen from scanning electron microscopy (SEM) images of the catalyst surface after growth (Fig. 2a). The gold catalyst adopts a {111} surface on the <001> sapphire substrate after annealing (Supplementary Fig. 1), leading to epitaxial growth of MoS2 across the catalyst surface. Low-energy electron diffraction (LEED) (Fig. 2c) and angle-resolved photoemission spectroscopy (ARPES) (Fig. 2d) of as-grown MoS2 domains on gold confirm uniform epitaxial alignment across the underlying substrate, as evidenced by the moiré satellite peaks visible in LEED25 and well resolved bands in ARPES. ARPES also indicates that the MoS2 domains are primarily monolayers, based on the absence of a strong anti-bonding band at the Γ point that is characteristic of multilayer formation26,27. Raman spectroscopy with 455 nm excitation of MoS2 crystals transferred to an oxidised silicon substrate shows two peaks, the E2g and A1g at 381.40 ± 0.05 and 401.40 ± 0.04 cm−1 respectively (Fig. 2e). While the positions and intensities of these peaks can in general vary as a result of strain and doping, their separation of ≈ 20 cm−1 is diagnostic of monolayer MoS228.

Fig. 2.

Fig. 2

Characterisation of MoS2. a SEM image of an individual MoS2 domain on Au {111} catalyst. Scale bar 1 µm. b SEM of epitaxially oriented MoS2 domains on gold. Scale bar 1 µm. c LEED pattern and d ARPES of as-grown MoS2 on Au {111}. The dashed lines in d serve as visual markers of the valence band of monolayer MoS2 at the K point of the Brillouin zone. e Raman response with 455 nm excitation of MoS2 transferred onto 90 nm SiO2/Si substrate. Two peaks are evident, the E2g peak at 381.40 cm−1 and the A1g at 401.40 cm−1

High resolution transmission electron microscopy (TEM) and selected area electron diffraction (SAED) images of crystals transferred to holey carbon support grids confirms the crystal structure of the MoS2 layers (Fig. 3a, b) and that the layers are free of atomic defects over the areas imaged. A region where vacuum is visible through the sample due to knock-on damage is indicated in Fig. 3a, confirming that the suspended region is a monolayer.

Fig. 3.

Fig. 3

TEM characterisation of MoS2. a High-resolution TEM of suspended MoS2. A hole in the monolayer introduced by knock-on damage during imaging is indicated (white arrow), where lattice fringes are absent. The boxed region has had an iterative nonlinear denoising filter applied to highlight the MoS2 lattice and reduce shot noise50. Scale bar 2 nm. b SAED pattern of suspended MoS2 layers with a 100 nm diameter aperture showing single crystal long range order. Scale bar 1 nm−1

Figure 4a shows photoluminescence (PL) measurements (see Methods) of MoS2 domains transferred onto 90 nm SiO2 on Si substrates (solid line), compared to a monolayer exfoliated MoS2 crystal control sample (dashed line). Identical acquisition parameters and substrates were used in both cases. The intensity of the PL response is comparable in both cases, while the PL peak for transferred crystals is blue-shifted with respect to exfoliated samples. Electric field-effect measurements were performed on 100 µm × 100 µm unencapsulated devices of continuous MoS2 films transferred onto 300 nm SiO2 on Si substrates with pre-patterned contacts (see Methods). Four-point sheet conductivity σS was calculated at varying gate bias (VG) as described in ref. 29, with the results for a representative device shown in Fig. 4b. The device shows an on-off ratio of >104 over the gate bias range, and small maximum hysteresis of about 16 V. The low level of hysteresis suggests that the overall number of charge traps is low, including intrinsic charge traps within MoS2 itself30. The field-effect mobility µ was calculated using the formula31 μ=(dσSdVG)1Cox, where Cox is the capacitance per unit area of the back gate. Our measured devices showed a range of µ between 5 and 30 cm2 V−1 s−1 (Supplementary Table 1), which is comparable to results for unencapsulated exfoliated MoS231.

Fig. 4.

Fig. 4

Photoluminescence and electrical characterisation of MoS2. a Photoluminescence spectra for the as-grown MoS2 transferred to SiO2 (solid line) vs. mechanically exfoliated monolayer MoS2 (dashed line). b Gate-dependent conductance measurements of a representative unencapsulated MoS2 device. Inset: image of a measured device. Scale bar 1 mm

Synthesis of other binary compounds

Varying M or X for a range of different elements (M = Mo, W, Cr, Fe, Co, Hf, Nb, V; X = S, Se, Te) under identical growth conditions results in the structures visible in the SEM images in Fig. 5. X-ray photoelectron spectroscopy (XPS) data confirming the expected stoichiometry and bonding for each of these binary transition metal dichalcogenides is presented in Supplementary Figs. 218, where further characterisation on selected materials is also presented. We have also shown the growth of select transitional metal nitrides, presented in Supplementary Figs. 1921, along with calculated band structures (Supplementary Fig. 22) for selected novel materials not present in the literature.

Fig. 5.

Fig. 5

Library of layered transition metal chalcogenides. SEM images of the various transition metal chalcogenides grown by the present method. All presented materials are grown under identical process conditions, varying only M and X. Further characterisation for the materials is presented in Supplementary Figs. 218. Scale bars are 1 µm except where marked: *: 100 nm, **: 10 µm

Discussion

We have shown the synthesis of epitaxially aligned MoS2 layers whose properties—namely Raman spectroscopic response, nanoscale crystalline structure, intensity of PL response, and electric field-effect properties—are comparable to mechanically exfoliated monolayers from bulk crystals or high-quality films from more complex CVD processes. This process is selective towards monolayer synthesis despite the fact that the solubility of molybdenum in gold is appreciable (~1 at%) at 850 °C17, demonstrating that the strict insolubility of all component elements is not required when extending surface-limited growth models to multi-elemental 2D compounds.

Furthermore, we show XPS and SEM data for a wide range of other materials produced simply by selecting different pairs of M and X elemental precursors, and additional Raman, atomic force microscopy (AFM), PL, and TEM characterisation for the materials which are stable during transfer to oxidised silicon or on the catalyst layer. Without further optimisation, a large selection of materials which display morphologies, stoichiometries, and chemical bonding expected of binary 2D transition metal dichalcogenides can be grown. While exhaustive characterisation of all of these materials is beyond the scope of this manuscript—in particular for candidate materials which have not previously been synthesised or isolated from bulk crystallites before—the simplicity of this growth strategy enables very rapid experimentation in terms of the range of precursor combinations that can be tested and materials which can be grown. In practice since multiple M-Au alloy samples can be simultaneously exposed to the same X precursor, the time needed to fully characterise such materials individually far exceeds the time needed to produce them in parallel.

The surface-limited growth of a wide variety of binary 2D materials presented in this work relies on the use of gold as a catalyst layer. Gold readily alloys with most transition metals M, but shows limited solubility for X elements at our growth temperatures. Moreover, gold is unique in that it does not react with X precursors at these temperatures. Gold is catalytically active, which aids in the formation of crystalline atomically thin materials, and the {111} surface formed on c-plane sapphire also templates the epitaxial alignment of the grown materials. The method presented here is distinct from vapour–liquid–solid (VLS) and vapour–solid–solid (VSS) growth models32 of III–V nanowires since we actively avoid supersaturation of component metals in gold—a key hallmark and necessary prerequisite for VLS/VSS growth mechanisms—by limiting the amount of metal available to <5 at%. This ensures that the resulting alloy behaves as a single-phase, simple solid solution at the growth temperature. The role of the gold here is to facilitate phase separation of M and X precursors such that they react only at the vapour–solid interface. Once this interface has been passivated by the 2D MXn layer, the growth terminates, similar to the case of graphene on copper.

The use of gold as a catalyst for synthesising 2D TMD layers has been previously reported in literature12,13,3335; however, a key advantage of the present scheme is that solid elemental metal films are used as precursors rather than metal-organic vapours or volatile metal compounds, which makes our process significantly simpler to implement for both known and new TMDs. We also note that similar methods for growing atomically thin carbides and sulphides have been previously reported36,37, but only for systems where both M and X components have limited solubility (<0.1 at%) in the catalyst. These represent a subset of the general approach presented here, i.e. one where the solubility of M in the catalyst approaches zero. In such cases, growth is dominated by surface-mediated diffusion of both M and X. Here instead the growth is dominated by precipitation of component M from the catalyst bulk upon reacting with X at the solid–gas interface at the surface of the catalyst. The crucial point is that surface-limited growth does not require the metal precursor to be insoluble in the catalyst layer. This fact allows our approach to be compatible with all precursor metals, in contrast to previous reports.

In the presented work, growth targeted at complete MoS2 monolayer coverage—achieved here by increasing the growth temperature—can result in adlayers. In practice, adlayer growth can be reduced by tuning the growth temperature and time, reducing the flux of X, or limiting the alloy M content of the gold catalyst layer. Controlling the M content can be particularly important in determining the layer coverage, maintaining single-phase alloying conditions, and in preventing precipitation of excess metal upon cooling. Such precipitation can interfere with 2D growth and lead to 3D structures on the surface, as seen for Co21 or Fe20. In general we expect that optimisation of additional deposition and growth parameters for individual MX combinations will be necessary, as has been the case for growth strategies for other 2D materials.

The present approach holds a number of advantages over state-of-the-art salt-assisted38 or metal-organic chemical vapour deposition (MOCVD) of 2D materials11. Notably, solid elemental precursors (elemental metal thin films; vapour phase S, Se, or Te) or simple compounds (NH3) are the only feedstocks required to grow the presented materials, which are in general more readily available and easier and safer to handle than metal-organic precursors and lead to less contaminants (such as carbon) being incorporated into the films. Critically, this approach provides a universal method for epitaxial synthesis of 2D materials without the need for salt additives38, which may have a detrimental impact on material performance through loss of epitaxy and alkali metal doping39. While we have employed a tube furnace operating under low pressure, the growth scheme presented does not rely on a flow but simply the presence of X precursor and as such can be performed in a sealed chamber. Such a scheme might be particularly beneficial to reduce the amount of oxygen and water in the growth system—the alloys of certain transition metals (e.g. Cr, Ta, Nb, Hf, V) are highly sensitive to oxidising impurities in the growth chamber40,41, which can interfere with growth by passivating the catalyst surface with metal oxides. This issue can be addressed by operating in a highly reducing environment or under high vacuum.

Some of the materials grown are unstable under ambient conditions—no special steps were taken to limit the exposure of samples to ambient atmosphere before characterisation. As such, transfer of many of these materials to, e.g., oxidised silicon substrates or TEM grids is challenging, as they rapidly degrade on contact with aqueous or oxygen-containing solutions, which has hampered extended characterisation in many cases. Recent progress in the solution-phase exfoliation of air and water-sensitive 2D crystals4244 suggests that similar strategies might be successfully employed here.

Conclusion

In summary, we have demonstrated a simple and universal strategy for approaching the growth of few-atom thick binary compounds, including transition metal mono- and dichalcogenides and nitride MXenes, based on the insight that only one component of a binary compound need be insoluble to achieve surface-limited growth. The strategy employs only a volatile X precursor, while all the presented materials are grown under identical conditions. Notably, this method enables the growth of epitaxially oriented MXn layers on Au. New 2D materials can be made through the free choice of M and X, and different compounds can be obtained on the same growth substrate simply by switching the precursor X gas. As such, this scalable growth technique simplifies the production of existing binary 2D materials with a quality comparable to exfoliated crystals, and at the same time greatly increases the range of such materials available. We do not doubt that growth conditions for materials can be individually optimised, and that with further research, growth of in-plane and out-of-plane heterostructures could also be accessible.

Methods

Preparation of gold-metal M substrates

Substrates were prepared by physical vapour deposition of a thin layer (~20 nm) of metal M followed by a thick layer (between 300 nm–1 µm, typically ~500 nm) of gold (Lesker, 99,999%) on a <001> sapphire substrate. Oxidation of the metal M is avoided by immediate encapsulation with gold before exposure to ambient conditions.

Synthesis of 2D transition metal chalcogenides and nitrides

Transition metal chalcogenides were synthesised in a hot-wall quartz tube reactor under low-pressure conditions. The chamber was flushed three times with argon (Ar), and the samples were subsequently heated to 850 °C under 100 sccm Ar. The samples were annealed at this temperature for 30–60 min, and growth was subsequently carried out for 10–15 min by exposing the samples to volatised chalcogen X vapours. The vapours were generated by heating solid chalcogen precursors situated upstream from the samples: ~110 °C for sulphur (sulphur flakes; Sigma Aldrich), ~220 °C for selenium (selenium pellets; Sigma Aldrich), and ~420 °C for tellurium (tellurium pieces; Sigma Aldrich). After growth, the samples were naturally cooled to room temperature under 100 sccm Ar flow. Synthesis of continuous MoS2 films for electrical device measurements was achieved by increasing the growth temperature to 950 °C.

Identical processing conditions were used to synthesise transition metal nitrides in a cold-wall reactor (AIXTRON Black Magic), except that the entire process was done under 100 sccm H2 flow instead of argon in order to mitigate surface oxidation of the alloys. The growth of nitrides was performed by introducing 5 sccm NH3 into the chamber for 5 min The samples were then naturally cooled down to room temperature under 100 sccm H2.

Transfer of 2D materials

Samples were transferred from the gold substrate by etching transfer. A solution of 10% wt. PMMA 950K in anisole (Sigma Aldrich) was spincoated onto the samples at 1500 rpm for 1 min, after which the samples were baked at 160 °C for 15 min. The polymer film was then manually removed at the edges of the sample. The samples were then put in a KI/I2 gold etchant solution (standard gold etchant; Sigma Aldrich). After the gold was completely etched, the films were washed in DI water and transferred onto oxidised silicon substrates, where they were baked at 160 °C for 10 min. PMMA was subsequently removed in acetone. Transfer of 2D materials onto TEM grids (Quantifoil GmbH) was done by wedging transfer45,46 from transferred films on oxidised silicon.

Crystal and band structure characterisation

SEM images were taken in a Zeiss Supra 40VP operated in in-lens detection mode at 5 keV. TEM characterisation of transferred MoS2 was done in an FEI Tecnai T20 G2 operated at 200 kV. ARPES and LEED measurements were conducted at the SGM-3 beamline endstation at ASTRID2 in Aarhus, Denmark. ARPES measurements for MoS2 were acquired at T = 30 K and hv = 49 eV, using an energy resolution <25 meV and angular resolution <0.2°47. LEED images were acquired at T = 30 K and EK = 113 eV.

Raman and PL measurements

Raman spectroscopy was conducted in a Thermo Fisher DXR microscope equipped with a 455 nm laser. Measurements were made using an incident power of 5 mW and a 50× objective, and 5 acquisitions with 10 s exposure time were collected for each Raman spectrum. Photoluminescence spectra were obtained using a custom spectroscopy setup built from a Nikon Eclipse Ti-U inverted microscope. The excitation source was a 407 nm diode laser from Integrated Optics. The light was focused to a diffraction limited spot on the sample with a TU Plan Fluor objective from Nikon (×100, 0.9 NA) resulting in an incident power of 30 µW. The emitted fluorescent light was collected with the same objective, and the spectra were recorded using a Shamrock 303i Spectrometer equipped with a 450 nm longpass filter (FELH0450 from Thorlabs) and an electronically cooled Newton 970 EMCCD. A total of five acquisitions with 1 s exposure time each were collected for each PL spectrum.

Fabrication of electrical devices

Continuous MoS2 films were transferred from the catalyst surface using the above procedure onto 300 nm SiO2/Si substrates with predefined electrical contacts48. Typical channel length was 100×100 µm2. Devices were electrically characterised in a Linkam LTS600P probe station after desorbing water from the surface49 via baking at 225 °C for 30 min in dry nitrogen. Subsequent measurements were performed under dry nitrogen at room temperature.

Supplementary information

Peer Review File (1.3MB, pdf)

Acknowledgements

A.S., J.D.T., P.R.W, T.J.B. and P.B. acknowledge support from the EU Seventh Framework Programme (FP7/2007–2013) under grant agreement number FP7-6040007 GLADIATOR. D.M.A.M., P.R.W., and P.B. acknowledge support from the EU Horizon 2020 Future and Emerging Technologies programme under grant agreement numbers 696656 and 785219. A.S., J.D.T, M.G., N.S., T.J.B. and P.B. acknowledge support from the Danish National Research Foundation Center of Excellence for Nanostructured Graphene (CNG) (project DNRF103). R.-M.S., A.J.H, M.B. and P.H. acknowledge the support from the Danish Council for Independent Research, Natural Sciences under the Sapere Aude program (grant no. DFF-4002-00029) and Villum Fonden under Center of Excellence for Dirac Materials (grant no. 11744). A. Crovetto acknowledges support from the Villum Fonden, research grant 9455. M.G. and N.S. acknowledge support from the Danish National Research Foundation IDUN Center of Excellence (project DNRF122) and Villum Fonden (research grant 9301) for partially funding the PL setup.

Author Contributions

A.S. conceived the method and performed the majority of the experiments. J.D.T. and T.J.B. performed TEM and SAED measurements. D.M.A.M. fabricated field-effect devices and performed electrical measurements. M.G. and N.S. performed and analysed photoluminescence measurements. R.-M.S., A.J.H, M.B., and P.H. performed LEED and ARPES characterisation. A. Crovetto did ellipsometry measurements. P.R.W. performed terahertz time domain spectroscopy measurements. A. Carvalho and A.H.C.N. provided band structure calculations. T.J.B. and P.B. supervised the project. T.J.B. and A.S. wrote the manuscript and prepared the figures, and all authors contributed to manuscript revisions.

Data Availability

The datasets generated during and/or analysed during the current study are available from the corresponding author on reasonable request.

Competing interests

A patent application has been filed and a PCT application has been published (WO 2018/087281 A1) by the Technical University of Denmark.

Footnotes

Peer review information: Nature Communications thanks the anonymous reviewer(s) for their contribution to the peer review of this work. Peer reviewer reports are available.

Publisher’s note: Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Supplementary information

Supplementary Information accompanies this paper at 10.1038/s41467-019-11075-2.

References

  • 1.Geim AK, Grigorieva IV. Van der Waals heterostructures. Nature. 2013;499:419–425. doi: 10.1038/nature12385. [DOI] [PubMed] [Google Scholar]
  • 2.Anasori B, Lukatskaya MR, Gogotsi Y. 2D metal carbides and nitrides (MXenes) for energy storage. Nat. Rev. Mater. 2017;2:16098. doi: 10.1038/natrevmats.2016.98. [DOI] [Google Scholar]
  • 3.Tan C, et al. Recent advances in ultrathin two-dimensional nanomaterials. Chem. Rev. 2017;117:6225–6331. doi: 10.1021/acs.chemrev.6b00558. [DOI] [PubMed] [Google Scholar]
  • 4.Miró P, Audiffred M, Heine T. An atlas of two-dimensional materials. Chem. Soc. Rev. 2014;43:6537–6554. doi: 10.1039/C4CS00102H. [DOI] [PubMed] [Google Scholar]
  • 5.Butler SZ, et al. Progress, challenges, and opportunities in two-dimensional materials beyond graphene. ACS Nano. 2013;7:2898–2926. doi: 10.1021/nn400280c. [DOI] [PubMed] [Google Scholar]
  • 6.Shi Y, Li H, Li L. Recent advances in controlled synthesis of two-dimensional transition metal dichalcogenides via vapour deposition techniques. Chem. Soc. Rev. 2015;44:2744–2756. doi: 10.1039/C4CS00256C. [DOI] [PubMed] [Google Scholar]
  • 7.Elías AL, et al. Controlled synthesis and transfer of large-area WS2 sheets: from single layer to few layers. ACS Nano. 2013;7:5235–5242. doi: 10.1021/nn400971k. [DOI] [PubMed] [Google Scholar]
  • 8.Lee Y-H, et al. Synthesis of large-area MoS2 atomic layers with chemical vapor deposition. Adv. Mater. 2012;24:2320–2325. doi: 10.1002/adma.201104798. [DOI] [PubMed] [Google Scholar]
  • 9.Lin Y-C, et al. Wafer-scale MoS2 thin layers prepared by MoO3 sulfurization. Nanoscale. 2012;4:6637–6641. doi: 10.1039/c2nr31833d. [DOI] [PubMed] [Google Scholar]
  • 10.Wang X, et al. Chemical vapor deposition growth of crystalline monolayer MoSe2. ACS Nano. 2014;8:5125–5131. doi: 10.1021/nn501175k. [DOI] [PubMed] [Google Scholar]
  • 11.Kang K, et al. High-mobility three-atom-thick semiconducting films with wafer-scale homogeneity. Nature. 2015;520:656–660. doi: 10.1038/nature14417. [DOI] [PubMed] [Google Scholar]
  • 12.Gao Y, et al. Large-area synthesis of high-quality and uniform monolayer WS2 on reusable Au foils. Nat. Commun. 2015;6:8569. doi: 10.1038/ncomms9569. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 13.Song I, et al. Patternable large-scale molybdenium disulfide atomic layers grown by gold-assisted chemical vapor deposition. Angew. Chem. Int. Ed. 2014;53:1266–1269. doi: 10.1002/anie.201309474. [DOI] [PubMed] [Google Scholar]
  • 14.Lee JS, et al. Wafer-scale single-crystal hexagonal boron nitride film via self-collimated grain formation. Science. 2018;362:817–821. doi: 10.1126/science.aau2132. [DOI] [PubMed] [Google Scholar]
  • 15.Li X, et al. Large-area synthesis of high-quality and uniform graphene films on copper foils. Science. 2009;324:1312–1314. doi: 10.1126/science.1171245. [DOI] [PubMed] [Google Scholar]
  • 16.Kidambi PR, et al. In-situ observations during chemical vapor deposition of hexagonal boron nitride on polycrystalline copper. Chem. Mater. 2014;26:6380–6392. doi: 10.1021/cm502603n. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 17.Massalski TB, Okamoto H. The Au-Mo (gold-molybdenum) system. Bull. Alloy Phase Diagr. 1986;7:449–452. doi: 10.1007/BF02867807. [DOI] [Google Scholar]
  • 18.Okamoto H, Massalski TB. The Au−W (gold-tungsten) system. Bull. Alloy Phase Diagr. 1985;6:136–137. doi: 10.1007/BF02869226. [DOI] [Google Scholar]
  • 19.Okamoto H, Massalski TB. The Au-Cr (gold-chromium) system. Bull. Alloy Phase Diagr. 1985;6:224–228. doi: 10.1007/BF02880403. [DOI] [Google Scholar]
  • 20.Okamoto H, Massalski TB, Swartzendruber LJ, Beck PA. The Au−Fe (gold-iron) system. Bull. Alloy Phase Diagr. 1984;5:592–601. doi: 10.1007/BF02868322. [DOI] [Google Scholar]
  • 21.Okamoto H, Massalski TB, Nishizawa T, Hasebe M. The Au-Co (gold-cobalt) system. Bull. Alloy Phase Diagr. 1985;6:449–454. doi: 10.1007/BF02869509. [DOI] [Google Scholar]
  • 22.Okamoto H, Massalski TB. The Au-Hf (gold-hafnium) system. Bull. Alloy Phase Diagr. 1984;5:379–380. doi: 10.1007/BF02872954. [DOI] [Google Scholar]
  • 23.Okamoto H, Massalski TB. The Au−Nb (gold-niobium) system. Bull. Alloy Phase Diagr. 1985;6:134–136. doi: 10.1007/BF02869225. [DOI] [Google Scholar]
  • 24.Predel, B. in Ac-Au–Au-Zr (ed. Madelung, O.) 1–4 (Springer-Verlag, Berlin, 1991).
  • 25.Grønborg SS, et al. Synthesis of epitaxial single-layer MoS2 on Au(111) Langmuir. 2015;31:9700–9706. doi: 10.1021/acs.langmuir.5b02533. [DOI] [PubMed] [Google Scholar]
  • 26.Zhang Y, et al. Direct observation of the transition from indirect to direct bandgap in atomically thin epitaxial MoSe2. Nat. Nanotechnol. 2013;9:111–115. doi: 10.1038/nnano.2013.277. [DOI] [PubMed] [Google Scholar]
  • 27.Miwa JA, et al. Van der Waals epitaxy of two-dimensional MoS2 – graphene heterostructures in ultrahigh vacuum. ACS Nano. 2015;9:6502–6510. doi: 10.1021/acsnano.5b02345. [DOI] [PubMed] [Google Scholar]
  • 28.Li H, et al. From bulk to monolayer MoS2: evolution of Raman scattering. Adv. Funct. Mater. 2012;22:1385–1390. doi: 10.1002/adfm.201102111. [DOI] [Google Scholar]
  • 29.Mackenzie DMA, et al. Quality assessment of graphene: continuity, uniformity, and accuracy of mobility measurements. Nano Res. 2017;10:3596–3605. doi: 10.1007/s12274-017-1570-y. [DOI] [Google Scholar]
  • 30.Kaushik N, et al. Reversible hysteresis inversion in MoS2 field effect transistors. npj 2D Mater. Appl. 2017;1:34. doi: 10.1038/s41699-017-0038-y. [DOI] [Google Scholar]
  • 31.Kim JH, et al. Thickness-dependent electron mobility of single and few-layer MoS2 thin-film transistors. AIP Adv. 2016;6:065106. doi: 10.1063/1.4953809. [DOI] [Google Scholar]
  • 32.Wagner RS, Ellis WC. Vapor-liquid-solid growth mechanism of single crystal growth. Appl. Phys. Lett. 1964;4:89–90. doi: 10.1063/1.1753975. [DOI] [Google Scholar]
  • 33.Shi J, et al. Controllable growth and transfer of monolayer MoS2 on Au foils and its potential application in hydrogen evolution reaction. ACS Nano. 2014;8:10196–10204. doi: 10.1021/nn503211t. [DOI] [PubMed] [Google Scholar]
  • 34.Yun SJ, et al. Synthesis of centimeter-scale monolayer tungsten disulfide film on gold foils. ACS Nano. 2015;9:5510–5519. doi: 10.1021/acsnano.5b01529. [DOI] [PubMed] [Google Scholar]
  • 35.Shi J, et al. Two-dimensional metallic tantalum disulfide as a hydrogen evolution catalyst. Nat. Commun. 2017;8:958. doi: 10.1038/s41467-017-01089-z. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 36.Xu C, et al. Large-area high-quality 2D ultrathin Mo2C superconducting crystals. Nat. Mater. 2015;14:1135–1141. doi: 10.1038/nmat4374. [DOI] [PubMed] [Google Scholar]
  • 37.Zhang T, et al. Twinned growth behaviour of two-dimensional materials. Nat. Commun. 2016;7:13911. doi: 10.1038/ncomms13911. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 38.Zhou J, et al. A library of atomically thin metal chalcogenides. Nature. 2018;556:355–359. doi: 10.1038/s41586-018-0008-3. [DOI] [PubMed] [Google Scholar]
  • 39.Zhang K, et al. Considerations for utilizing sodium chloride in epitaxial molybdenum disulfide. ACS Appl. Mater. Interfaces. 2018;10:40831–40837. doi: 10.1021/acsami.8b16374. [DOI] [PubMed] [Google Scholar]
  • 40.Tynkova A, Sidorenko S, Voloshko S, Rennie AR, Vasylyev MA. Interdiffusion in Au (120 nm)/Ni (70 nm) thin films at the low-temperature annealing in the different atmospheres. Vacuum. 2013;87:69–74. doi: 10.1016/j.vacuum.2012.07.005. [DOI] [Google Scholar]
  • 41.Ashwell GWB. Interdiffusion of titanium and gold: a comparison of thin films deposited in technical vacuum and ultrahigh vacuum. J. Electrochem. Soc. 1981;128:649–654. doi: 10.1149/1.2127475. [DOI] [Google Scholar]
  • 42.Hanlon D, et al. Liquid exfoliation of solvent-stabilized few-layer black phosphorus for applications beyond electronics. Nat. Commun. 2015;6:8563. doi: 10.1038/ncomms9563. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 43.Kang J, et al. Solvent exfoliation of electronic-grade, two-dimensional black phosphorus. ACS Nano. 2015;9:3596–3604. doi: 10.1021/acsnano.5b01143. [DOI] [PubMed] [Google Scholar]
  • 44.Kang J, et al. Stable aqueous dispersions of optically and electronically active phosphorene. Proc. Natl. Acad. Sci. USA. 2016;113:11688–11693. doi: 10.1073/pnas.1602215113. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 45.Schneider GF, Calado VE, Zandbergen H, Vandersypen LMK, Dekker C. Wedging transfer of nanostructures. Nano. Lett. 2010;10:1912–1916. doi: 10.1021/nl1008037. [DOI] [PubMed] [Google Scholar]
  • 46.Thomsen JD, et al. Suppression of intrinsic roughness in encapsulated graphene. Phys. Rev. B. 2017;96:014101. doi: 10.1103/PhysRevB.96.014101. [DOI] [Google Scholar]
  • 47.Hoffmann SV, Søndergaard C, Schultz C, Li Z, Hofmann P. An undulator-based spherical grating monochromator beamline for angle-resolved photoemission spectroscopy. Nucl. Instrum. Methods Phys. Res. Sect. A. 2004;523:441–453. doi: 10.1016/j.nima.2004.01.039. [DOI] [Google Scholar]
  • 48.Mackenzie DMA, et al. Graphene antidot lattice transport measurements. Int. J. Nanotechnol. 2017;14:226. doi: 10.1504/IJNT.2017.082469. [DOI] [Google Scholar]
  • 49.Gammelgaard L, et al. Graphene transport properties upon exposure to PMMA processing and heat treatments. 2D Mater. 2014;1:035005. doi: 10.1088/2053-1583/1/3/035005. [DOI] [Google Scholar]
  • 50.Du H. A nonlinear filtering algorithm for denoising HR(S)TEM micrographs. Ultramicroscopy. 2015;151:62–67. doi: 10.1016/j.ultramic.2014.11.012. [DOI] [PubMed] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Peer Review File (1.3MB, pdf)

Data Availability Statement

The datasets generated during and/or analysed during the current study are available from the corresponding author on reasonable request.