Skip to main content
Microsystems & Nanoengineering logoLink to Microsystems & Nanoengineering
. 2020 Nov 16;6:102. doi: 10.1038/s41378-020-00212-3

Sensitive capacitive pressure sensors based on graphene membrane arrays

Makars Šiškins 1,, Martin Lee 1, Dominique Wehenkel 2, Richard van Rijn 2, Tijmen W de Jong 1, Johannes R Renshof 1, Berend C Hopman 1, Willemijn S J M Peters 1, Dejan Davidovikj 1, Herre S J van der Zant 1, Peter G Steeneken 1,3,
PMCID: PMC8433463  PMID: 34567711

Abstract

The high flexibility, impermeability and strength of graphene membranes are key properties that can enable the next generation of nanomechanical sensors. However, for capacitive pressure sensors, the sensitivity offered by a single suspended graphene membrane is too small to compete with commercial sensors. Here, we realize highly sensitive capacitive pressure sensors consisting of arrays of nearly ten thousand small, freestanding double-layer graphene membranes. We fabricate large arrays of small-diameter membranes using a procedure that maintains the superior material and mechanical properties of graphene, even after high-temperature annealing. These sensors are readout using a low-cost battery-powered circuit board, with a responsivity of up to 47.8 aF Pa−1 mm−2, thereby outperforming the commercial sensors.

Subject terms: Nanosensors, NEMS, Sensors

Sensors that perform well under pressure

Arrays of tiny graphene membranes exhibit excellent performance as pressure sensors, offering a competitive, low-cost alternative to commercially available systems. Graphene offers a durable and resilient material for sensors that generate a capacitive readout to pressure changes, but individual membranes are not sufficiently sensitive. Researchers led by Makars Šiškins and Peter Steeneken of the Delft University of Technology in the Netherlands have devised a strategy for fabricating graphene sensor arrays that overcome this limitation. Their method yields millimeter-scale assemblies of 10,000 double-layered graphene membranes, which can in turn be connected to an inexpensive battery-powered circuit board. The authors demonstrate that this system can outperform a state-of-the-art commercial pressure sensor, and propose that further improvements to the design and fabrication of these arrays could improve their responsiveness by a full order of magnitude.

Introduction

Graphene grown by chemical vapor deposition (CVD) is a strong candidate for realizing next-generation sensor devices1. Its hermeticity24 and superior mechanical57 and electrical8 properties have enabled various types of gas pressure sensors. In most conventional pressure sensors, the pressure is determined from the deflection of a membrane due to the pressure difference between ambient gas and gas in a hermetically sealed reference cavity. There are different ways to readout the deflection of the membrane and thereby quantify the pressure difference. In capacitive graphene pressure sensors, the deflection is readout by measuring the capacitance between the graphene membrane and a reference electrode912. As the pressure-induced deflection increases the mechanical stress and tension in the membrane, it can be measured using the piezoresistive effect1315 and can be probed via the mechanical resonance frequency2,3,16. In contrast, graphene squeeze-film pressure sensors17 and Pirani pressure sensors18 do not require a hermetic reference cavity and operate at small deflection, which can be beneficial for their operation range.

Resonant sensors are conceptually attractive because they potentially offer both gas sensing19,20 and pressure sensing2,17 functionality within a single device. However, the accurate readout of resonance frequencies with low-power electronics is challenging, requires the elimination of mass loading and cannot be easily scaled up to many devices in parallel. In piezoresistive and Pirani sensors, it is a challenge to eliminate nonpressure-related effects of the surrounding gas on the graphene resistance. In contrast, capacitive pressure sensors have the advantage that the membrane capacitance is rather insensitive to gas-induced changes in its mass and electrical resistance and thus depends mainly on the geometry and membrane deflection. However, it was found that a single graphene membrane with a diameter of 5 μm has too small of a responsivity (<0.1 aF Pa−1) to be competitive with commercial sensors12.

In this work, we counter this drawback by creating arrays with a large number of membranes connected in parallel to increase the responsivity12. We present few-atom-thick pressure sensors that can compete with commercial capacitive pressure sensors using arrays of nearly 10,000 double-layer graphene (DLG) membranes. We optimize the design of the sensor elements, the chip layout and the readout electronics to attain a handheld, low cost, battery-powered electrical readout circuit capable of detecting pressure changes via the static deflection of graphene nanodrums.

Materials and methods

Chip design and graphene transfer

Simulations12 have shown that to achieve commercially competitive sensitivity, an array of ~10,000 circular graphene drums is needed, each with a diameter of 5 microns. When the drums are placed on a hexagonal grid with a pitch of 10 microns between their centers, they fit on a 1×1 mm2 chip, as shown in Fig. 1a. To fabricate this design, Ti/Au electrodes (5 nm/60 nm), for contacting the graphene top electrode, are patterned on a silicon chip with a 285 nm SiO2 layer. Then, the pattern of circular holes with a depth of 240 nm is reactive ion etched into the SiO2. As shown in the cross-section in Fig. 1b, the cavity depth of the holes is less than the SiO2 layer thickness to prevent the graphene from touching the silicon bottom electrode, which would create an electrical short-circuit between the electrodes if one of the membranes collapses. As a last step, the graphene is transferred over the cavities. We use two layers of graphene and a small membrane diameter to improve the yield21 and the mechanical strength7,22. Since the probability that 2 pore defects align is low, the impermeability of DLG is also much higher than that of single-layer graphene3.

Fig. 1. Pressure sensor and readout circuitry.

Fig. 1

a Optical image of the sensor chip with 10,000 circular holes, a DLG/PMMA membrane and Ti/Au electrodes. The close-up image shows the difference in contrast between intact and defect drums, with red circles indicating collapsed membranes. b Schematic device cross-section and capacitive pressure readout principle. c Readout circuitry PCB board, with the elements labeled. The total size of the PCB board is 6.9×17.5 cm2. The red circle indicates the pressure sensor chip

To fabricate DLG, two sheets of CVD graphene are synthesized and then stacked on top of each other, maintaining a pristine quality interface between the sheets. Using polymethyl methacrylate (PMMA) as a support layer of 800 nm thickness, DLG is suspended over the prepatterned circular holes in the SiO2/Si chip with Ti/Au electrodes (Fig. 1a). The DLG was produced and transferred to ambient pressure by Applied Nanolayers. From the differences in contrast between suspended, broken and collapsed drums21,23 we estimate that the dry transfer technique results in a yield of 9599% of freely suspended DLG/PMMA membranes. The red circles in the inset of Fig. 1a indicate defect drums in a damaged region of the sample and show this difference in contrast.

Sensor readout circuit board

The graphene capacitive pressure sensor responds to the difference established between the internal pressure of the reference cavity, Pint, and the external pressure of the environment, Pext. This pressure difference results in a deflection of the atomically thin membrane and a corresponding change in capacitance12 of the drum, ΔC, as schematically depicted in Fig. 1b. We wedge-bond a 25 μm AlSi 1% wire to Ti/Au pads on a chip for electrical contact with graphene and use a conductive silver paste to contact the Si substrate. The response of the graphene capacitive pressure sensor is high enough to be readout by chip-scale commercial electronic components, as demonstrated using the battery-powered circuit shown in Fig. 1c. Here, the sample under test is kept in a small on-board vacuum chamber that allows local control over the external gas pressure while preventing the pressure from affecting the electrical readout elements. A commercial capacitance to digital converter (AMS PCap04) is then used to record and digitize the capacitance of the sample measured at a peak-to-peak voltage Vpp=1.5 V with a hundred charge and discharge cycles of 5.73 ms each. After voltage level adjustment by a logic level converter, an Arduino Uno board converts the measured capacitance into pressure using a predetermined calibration curve and displays it on an LCD screen. The circuit board is capable of measuring a change in the chip’s capacitance down to ~10 aF on top of a background capacitance of a few tens of picofarads.

Effect of PMMA removal

After chip fabrication and transfer, the PMMA transfer polymer still covers the DLG sheets. In a number of previous studies, protective polymer layers were used to support graphene to increase the yield, mechanical performance, hermeticity, and durability of the devices in both suspended10,24 and touch-mode11 operation. However, the bending rigidity of the polymer layers reduces the deflection and responsivity of the membranes and sensor. To improve the sensor performance, we therefore gradually remove the transfer polymer by annealing it in dry gas2528 as shown in Fig. 2. PMMA removal mechanisms are mostly related to removing pendant functional groups in the polymer at high temperatures25,27. However, this can trigger a reaction between the graphene and the carbon byproducts from the residual polymer and produce amorphous carbon25,26. Lower process temperatures and an atmosphere of inert gas, such as argon, are needed to prevent the production of amorphous carbon and to maintain a good quality of graphene during thermal annealing26.

Fig. 2. Thermal removal of the polymer and its effect on the capacitive response of the sensor.

Fig. 2

a Schematic explanation of the thermal annealing principle applied to reduce the PMMA thickness h(t). b Change in capacitance of a single chip as a function of measurement in response to time-dependent pressure changes, ΔP, for samples that have been annealed for different times t (line colors correspond to the color of the corresponding annealing times indicated in the legend). The gas pressure is changed at a rate of 175.4 mbar s−1. c Responsivity and noise floor extracted from the data in b, calculated using Eq. (1)

The sample is placed inside a furnace and left at a pressure of 500 Torr with a constant flow of 0.5 SLPM of an inert dry gas (Ar or N2) at a temperature of 300C, as schematically depicted in Fig. 2a. We found no notable difference between the use of Ar or N2 gas flow in terms of the end quality of the DLG layers or the PMMA removal rate. The average thickness of the transfer PMMA decreases with annealing time at an estimated rate of ~27 nm/min, with only minor residues left on and in-between the graphene layers. For some samples, small regions of local PMMA residue accumulation are still present after the annealing procedure. They accumulate on the surface of a DLG layer that has a thickness of 1.42.2 nm, as measured by tapping mode atomic force microscopy (AFM) (see Fig. S1). The PMMA thickness reduction by thermal treatment is found to substantially improve the responsivity of the sensors. Figure 2b shows the capacitance change ΔC of a single chip to external pressure changes between 1000 and 900 mbar with a period of 40 s, as measured after 0, 15, 22.5, and 29 minutes of annealing. Figure 2c shows that by following the thermal annealing procedure, an increase in responsivity of almost an order of magnitude was achieved for this particular sample, while in the best case, an increase in responsivity of nearly two orders of magnitude was observed after a 30 min continuous thermal annealing treatment. Further annealing of the sample for longer times does not significantly affect the capacitance response (see Fig. S2). The detection noise floor also decreases substantially as a result of the process. The noise floor, NF, in Pa/Hz is defined as:

NF=CRMSdCdPfmeas 1

where CRMS is the root mean squared (RMS) noise in the capacitance measurement, dCdP is the responsivity of the sensor and fmeas=1.745 Hz is the frequency at which the measurements are acquired. The decrease in NF, as shown in Fig. 2c, qualitatively follows from Eq. (1) considering the measured increase in responsivity.

Results and discussion

Sample characterization

After thermal treatment for 30 min at 300C, we inspect the samples for damage. In Fig. 3a, a tapping mode atomic force microscopy (AFM) image of the sample is shown. Three types of drums can be distinguished visually: intact, ruptured, and collapsed drums. Collapsed drums are in contact with the bottom of the cavity and probably do not significantly contribute to the response11 because they are predominantly damaged and thus not airtight. The ruptured drums are also expected to leak fast17 and therefore have a negligible contribution to the static capacitance response to gradual pressure changes. Intact drums, however, show full coverage of the cavity. These drums can hermetically seal the cavity with a constant internal pressure, exploiting the extremely low permeability of graphene24 although in part of these membranes, small pores can be present that are too small to be visually detected. The lower height of some drums visible in Fig. 3a can be caused by the small downward pressure or Pint<1 bar established during the fabrication process. As shown in the AFM measurements in Fig. 3b, after the annealing process, a substantial number of residues are observed on and below the DLG. The residues form pockets and are also observed in the suspended regions of the device, which suggests that parts of the residues are trapped in-between the graphene layers, where they cannot be easily removed29.

Fig. 3. Atomic force microscopy (AFM) characterization of membranes.

Fig. 3

a AFM tapping mode image of DLG drums. The state of the drum is labeled. Scale bar: 5 μm. b AFM tapping mode image of a supported region of DLG. Residue types are indicated. Scale bar: 1 μm. c Force versus membrane deflection curve. Experimental data (blue dots) are fit by the membrane model of Eq. (2). Inset: statistics over 21 membranes with the corresponding mean values for the extracted two-dimensional Young’s modulus, E2D, with a mean pretension n0=0.04±0.02 N/m

During fabrication, the capability of graphene to withstand high strains5,6,30 facilitates damage-free transfer, while the thickness of only a few atoms favors higher membrane deflections and thus higher responsivity to pressure changes of the sensor. To test the elasticity and mechanical properties of the drums after thermal treatment, we use force-indention AFM to apply a point force at the center of a single membrane while measuring its deflection5. The applied force, F, is proportional to the stiffness of a cantilever kc and its deflection Δzc as F=kcΔzc. We use two cantilevers of kc=1.25±0.12 N/m and 1.48±0.05 for two separate sets of measurements in two distant places on the chip. We record a force versus membrane deflection curve at the center of each drum, as depicted in Fig. 3c, and fit it to a model of the point deflection of a circular membrane5,31:

F=n0πδ+E2DRq3δR3 2

where n0 is the pretension, E2D is the two-dimensional Young’s modulus of the layer, ν=0.16 is Poisson’s ratio7, δ is the resulting deflection, R is the radius and q=1/1.050.15ν0.16ν2 is a geometrical factor5,31. We use the two-dimensional Young’s modulus, E2D=E3Dh, for the stacked DLG sheet since the thickness, h, of the layer after the thermal treatment is not well defined. This effective quasi-2D Young’s modulus provides a more realistic estimate for the mechanical elasticity of the layer and can be directly compared to that of pristine single-layer graphene5. In the inset of Fig. 3c, the statistics over 21 different drums, which yield a mean value of E2D=175 N/m, are shown. This mean value is substantially lower than the reported values for both exfoliated and pristine CVD single-layer graphene5,7 but comparable to those of other CVD graphene membranes24,30,32,33, high-quality oxidized graphene sheets34,35 and other 2D materials such as single-layer MoS231.

We also examined the sheets of DLG by using Raman spectroscopy, as displayed in Fig. 4. Figure 4a shows Raman spectra of DLG acquired before the removal of the PMMA layer (blue line) and after processing at an elevated temperature (orange and magenta line). Before the thermal treatment, the Raman spectrum of the DLG is reasonably homogeneous across the chip, showing a Lorentzian-shaped 2D peak of graphene and a well-defined G peak36. The full width at half maximum (FWHM) of the 2D peak is ~30 cm−1, and the high intensity ratio of 2D to G peaks resembles typical features of pristine graphene36. In the case of DLG, this result indicates that the two layers in the stack are well decoupled and/or have, on average, a twist angle37 larger than 15. After processing at a high temperature, the width of the 2D peak remains the same (see Fig. 4b), while the ratio of 2D to G peaks changes drastically depending on the chosen location of the measurement on the chip (see Fig. 4a, orange and magenta lines). Additionally, a notable blueshift of both the 2D and G peaks is observed, as shown in Fig. 4b, c. These observations are attributed to a substantial difference in the twist angle across the DLG sheet37 as well as local changes in strain as a result of annealing of the graphene layers38.

Fig. 4. Raman spectroscopy of supported DLG.

Fig. 4

a Raman spectra of the DLG/PMMA layer before and after polymer removal. b Close-up of a blueshift in the 2D peak and c the G peaks of graphene

We also note the almost complete absence of the D peak in all Raman spectra, as shown in Fig. 4a, indicating a very low amount of defects in the stacked graphene layers even after exposure to high temperatures39. This result is in agreement with the outstanding high-temperature stability of graphene when encapsulated by protective layers40,41 and provides evidence that damage caused by the removal of polymer from suspended graphene is minimal2528.

Analysis of the sensor response

A pressure difference ΔP results in a deflection δ of a circular graphene membrane with radius R, given by:

ΔP=4n0R2δ+8E2D3R4(1ν)δ3 3

where the graphene membrane takes the shape of the section of a sphere12,42. Since the pressure inside the reference cavity is approximately Pint1 bar (the pressure during transfer), at Pext=1 bar (atmospheric pressure, ΔP0) and according to Eq. (3), the sensors are expected to have a linear response at small Δδ. However, at larger deflections, nonlinear mechanical and capacitance effects start to result in nonlinearities in the capacitance Cd(ΔP) curve that can be calculated using the parallel-plate approximation12 as:

Cd(ΔP)=2πϵ00Rrg0δ(ΔP)1r2R2dr 4

where ϵ0 is the vacuum permittivity and g0 is the gap size between the membrane and bottom electrode for ΔP=0. The contribution of the quantum capacitance of graphene is small43,44 and is neglected. The total capacitance change of the sensor can be modeled from Eqs. (3) and (4) as:

ΔCtotal=N×ΔCd(ΔP) 5

where N is the number of intact, hermetic drums after both fabrication and thermal treatment. We experimentally test whether Eqs. (4) and (5) can model the graphene pressure sensor by applying both substantial negative and positive pressure differences while measuring its capacitance. Figure 5a shows the response of the same sensor that was characterized in Figs. 3 and 4.

Fig. 5. Capacitance-pressure curves of the DLG pressure sensor.

Fig. 5

a Measured capacitance-pressure curve (blue points); solid magenta line is a fit of Eq. (5) to the data, with Pint=0.933 bar, N/Ntot = 0.25, E2D = 175 N/m and n0=0.45 N/m. Insets: schematic images of the effect of membrane deflection. b Comparison, on a log-scale, of the measured data (blue points) to the model with 100% (magenta dashed line) and 25% (solid magenta line) yield of the hermetic drums using the 2D Young’s modulus from Fig. 3. All data are acquired during a continuous measurement within a total time of 1 h at PextPint with a maximal rate of change of the gas pressure of 3.3 mbar s−1

The maximal responsivity of the sensor is achieved near ambient pressure in the linear regime, while a notable nonlinear response occurs for ΔP>200 mbar. A number of design factors, such as the drum diameter, the number of drums and the pitch between the drums, influence the sensor performance12. Importantly, the pressure dependence of ΔC can be well reproduced by the model of Eq. (5) using a Young’s modulus E2D=175 N/m, estimated by an AFM probe for this particular sample, and a pretension n0=0.45 N/m, as shown by the magenta line in Fig. 5a. The model follows the measurement closely when we use a fitted value of N/Ntot = 0.25, as shown in Fig. 5b (solid magenta line), where Ntot10000 is the total number of drums. This result indicates that the yield of intact hermetic drums is 25% and suggests that a large number of drums that look visually intact do not remain hermetic after polymer removal. The theoretical maximum response at a perfect yield of 100% is also shown (dashed magenta line).

Many other factors can influence the responsivity. Since the device capacitance has a strong dependence on the distance between the plates of the pressure sensor, the cavity depth has a large influence on the performance of the sensor. In Fig. 6, we demonstrate the performance of two of the best samples with SiO2 thicknesses of 285 nm and 2.17 μm. Both chips have circular holes with a depth of 240 nm fabricated as described previously. Figure 6a shows the triangular wave response of both 285 nm (orange line) and 2.17 μm (blue line) chips. As shown in Fig. 6b, the difference in responsivity for the two oxide thicknesses as a function of pressure can be more than an order of magnitude. Using Eq. (1), we calculate the noise floor to be 34.2 Pa/Hz for the 285 nm thick SiO2 sample and 43.4 Pa/Hz for the 2.17 μm sample. The measured responsivity of the 285 nm gap device is significantly higher than that of the 2.17 μm device, in qualitative accordance with Eq. (1).

Fig. 6. Comparison of different capacitive pressure sensors.

Fig. 6

a Triangular pressure wave applied to two graphene sensors with 285 nm and 2.17 μm oxide thickness, showing the measured change in capacitance. The gas pressure is changed at a rate of 6.25 mbar s−1. b Responsivity analysis of the chips at small ΔP using multiple periods of measured data from a as a function of the pressure change, and a comparison to a commercial capacitive pressure sensor (Murata SCB10H). c Analysis of the responsivity of the chips as determined from periodic pressure steps between 1000 and 900 mbar. The gas pressure is changed at a rate of 175.4 mbar s−1. Panels on the left: Blue line—measured capacitance of a graphene sensor with tSiO2=2.17 μm. Orange line—measured capacitance of a sensor with tSiO2=285 nm. Thin gray line—applied time-dependent pressure profile. Magenta lines—extracted capacitance response of the sensors. Panels on the right: statistics over a number of cycles for both oxide thicknesses. The higher responsivity and larger gas leak rate of the 285 nm device can account for the larger variations. Magenta lines—fit to a normal distribution, with the corresponding mean values μ and standard deviations σ in aF Pa−1 indicated

There is a notable scatter in the measured capacitance values, as seen in Fig. 6b, which is attributed to the effect of gas escaping the cavities for part of the drums, thus causing ΔP to decrease with measurement time. It has been reported before that when graphene is suspended over a SiO2/Si cavity, it does not always form a perfect hermetic seal2,3. As recently shown by Lee, et al., most of the gas permeation in graphene drums occurs along the van der Waals interface between the 2D material and the substrate2. As a result of the contribution of this effect, an exponential decrease in C with measurement time is visible in Fig. 6c, in response to periodic pressure steps of ΔP=100 mbar. However, if good graphene crystallinity is preserved over large areas, the mean path that the gas needs to travel to escape the cavities becomes large, which increases the flow resistance of the gas channel and the permeation time constant2,20. This condition seems to be achieved across part of the sample because no significant hysteresis was observed during the slow pressure sweeps (>10 minutes per sweep) in Fig. 5a, b, suggesting that on the order of 25% of the drums maintain a constant internal pressure Pint for ΔP0, as supported by the fits in Fig. 5a, b.

Optimization of all parameters is required to achieve the best sensor performance for detecting very small pressure differences over an extended range of pressures. DLG pressure sensors show reproducible operation over a pressure range of 65138 kPa (see Fig. 5a). In terms of responsivity, our best sensor with 285 nm of SiO2 oxide (orange dots in Fig. 6a, b), with a responsivity of 47.8 aF Pa−1 mm−2 over the range of 90100 kPa, already outperforms the commercially available state-of-the-art Murata SCB10H sensor, with a responsivity of 28 aF Pa−1 mm−2 in the same range, as shown in Fig. 6b. This outcome is comparably larger than what was previously achieved with capacitive sensors based on atomically thin 2D membranes9,12 yet competitive with thicker suspended graphene-covered 140 nm PMMA sheets10, with a reported responsivity of 123 aF Pa−1 mm−2 over 080 kPa, using an area of 210 μm2 of tightly packed hexagonal membranes. However, if yields close to 100% and hermetic sealing of all the drums is realized, and if the pretension is decreased to ~0.04 N/m, the presented graphene-based 2D devices are expected to achieve a theoretical maximum responsivity of ~450 aF Pa−1 mm−2 near ambient pressure of 90100 kPa. Further design improvements might even be possible if the gap is reduced, the unsuspended area is minimized and the packing density of the membranes is increased. Using three or five layers of stacked graphene instead of two might help to improve the hermetic sealing issue but will result in a lower sensitivity (see Fig. S3). Increasing the diameter of drums, on the other hand, could compensate for this and produce an increase in responsivity (see Fig. S4); however, it could also decrease the yield21. We demonstrate the proof-of-concept operation of graphene pressure sensors under room temperature conditions (~23C). Eventually, the temperature-related effects, such as the expansion of gas inside the cavities, small variations in the dielectric constant of the gas as a function of temperature, and thermal expansion of the DLG and Si/SiO2 substrate, can potentially affect the capacitance-to-pressure conversion. For operation over an extended temperature range, these need to be excluded by combining the pressure sensor with a temperature sensor45, by using appropriate calibration and by sealing the drums under vacuum conditions.

Conclusions

Where previous studies have addressed some of the challenges related to realizing portable graphene gas pressure sensors, such as the pressure sensitivity, impermeability to gases and electrical readout, here, we bridged these studies by constructing a portable, battery-powered functional graphene pressure sensor that outperforms commercial devices. Using off-the-shelf systems for electronic readout and data processing, we enable capacitive readout of a 1×1 mm2 array of DLG pressure sensors. We realize sensor chips with a high yield of suspended membranes, resulting in a sensor responsivity of 47.8 aF Pa−1 mm−2. We demonstrate that thermal treatment is an effective measure for controllable thickness reduction of the support polymer layer, which leads to a significant performance improvement because the thin 2D material membranes are much more flexible than those with the support polymer. It is anticipated that further design and fabrication improvements and better control over the device yield can increase the responsivity by a factor of 10, thus enabling improvements in applications such as indoor navigation, altitude monitoring and activity monitoring, and can enable new applications such as presence detection.

Supplementary information

41378_2020_212_MOESM1_ESM.docx (3MB, docx)

SUPPLEMENTARY INFORMATION: Sensitive capacitive pressure sensors based on graphene membrane arrays

Acknowledgements

M.Š., M.L., H.S.J.v.d.Z., and P.G.S. acknowledge funding from the European Union’s Horizon 2020 research and innovation program under grant agreement numbers 785219 and 881603.

Author contributions

M.L. and D.D. designed and fabricated the Si/SiO2 chips. R.v.R. and D.W. fabricated and transferred the CVD graphene stack at Applied Nanolayers. B.V. M.Š., and M.L. realized thermal removal of the polymer. T.W.d.J., J.R.R., and D.D. designed the readout circuit board. M.Š., M.L., T.W.d.J., J.R.R., B.C.H., W.S.J.M.P., and D.D. performed the capacitance measurements. T.W.d.J., J.R.R., B.C.H., and D.D. analyzed the noise level of the sensors. W.S.J.M.P. and M.Š. performed the AFM measurements. W.S.J.M.P., M.Š., and M.L. modeled the response of the sensor. D.D., H.S.J.v.d.Z., and P.G.S. conceived and supervised the project. The manuscript was jointly written by all authors with a main contribution from M.Š. All authors discussed the results and commented on the manuscript.

Data availability

The manuscript has associated data in a data repository. The numerical data shown in figures of the manuscript can be downloaded from the Zenodo online repository at https://doi.org/10.5281/zenodo.4042077.

Conflict of interest

The authors declare that they have no conflict of interest.

Contributor Information

Makars Šiškins, Email: m.siskins-1@tudelft.nl.

Peter G. Steeneken, Email: p.g.steeneken@tudelft.nl

Supplementary information

Supplementary information accompanies this paper at 10.1038/s41378-020-00212-3.

References

  • 1.Zurutuza A, Marinelli C. Challenges and opportunities in graphene commercialization. Nat. Nanotechnol. 2014;9:730–734. doi: 10.1038/nnano.2014.225. [DOI] [PubMed] [Google Scholar]
  • 2.Lee M, et al. Sealing graphene nanodrums. Nano Lett. 2019;19:5313–5318. doi: 10.1021/acs.nanolett.9b01770. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 3.Bunch JS, et al. Impermeable atomic membranes from graphene sheets. Nano Lett. 2008;8:2458–2462. doi: 10.1021/nl801457b. [DOI] [PubMed] [Google Scholar]
  • 4.Sun PZ, et al. Limits on gas impermeability of graphene. Nature. 2020;579:229–232. doi: 10.1038/s41586-020-2070-x. [DOI] [PubMed] [Google Scholar]
  • 5.Lee C, Wei X, Kysar JW, Hone J. Measurement of the elastic properties and intrinsic strength of monolayer graphene. Science. 2008;321:385–388. doi: 10.1126/science.1157996. [DOI] [PubMed] [Google Scholar]
  • 6.Cui T, et al. Fatigue of graphene. Nat. Mater. 2020;19:405–411. doi: 10.1038/s41563-019-0586-y. [DOI] [PubMed] [Google Scholar]
  • 7.Lee G-H, et al. High-strength chemical-vapor-deposited graphene and grain boundaries. Science. 2013;340:1073–1076. doi: 10.1126/science.1235126. [DOI] [PubMed] [Google Scholar]
  • 8.Chen J-H, Jang C, Xiao S, Ishigami M, Fuhrer MS. Intrinsic and extrinsic performance limits of graphene devices on SiO2. Nat. Nanotechnol. 2008;3:206–209. doi: 10.1038/nnano.2008.58. [DOI] [PubMed] [Google Scholar]
  • 9.Chen Y-M, et al. Ultra-large suspended graphene as a highly elastic membrane for capacitive pressure sensors. Nanoscale. 2016;8:3555–3564. doi: 10.1039/c5nr08668j. [DOI] [PubMed] [Google Scholar]
  • 10.Berger C, Phillips R, Centeno A, Zurutuza A, Vijayaraghavan A. Capacitive pressure sensing with suspended graphene–polymer heterostructure membranes. Nanoscale. 2017;9:17439–17449. doi: 10.1039/c7nr04621a. [DOI] [PubMed] [Google Scholar]
  • 11.Berger C, et al. Touch-mode capacitive pressure sensor with graphene-polymer heterostructure membrane. 2D Mater. 2017;5:015025. doi: 10.1039/c7nr04621a. [DOI] [PubMed] [Google Scholar]
  • 12.Davidovikj D, Scheepers PH, van der Zant HSJ, Steeneken PG. Static capacitive pressure sensing using a single graphene drum. ACS Appl. Mater. Interfaces. 2017;9:43205–43210. doi: 10.1021/acsami.7b17487. [DOI] [PubMed] [Google Scholar]
  • 13.Zhu S-E, Ghatkesar MK, Zhang C, Janssen GCAM. Graphene based piezoresistive pressure sensor. Appl. Phys. Lett. 2013;102:161904. [Google Scholar]
  • 14.Smith AD, et al. Electromechanical piezoresistive sensing in suspended graphene membranes. Nano Lett. 2013;13:3237–3242. doi: 10.1021/nl401352k. [DOI] [PubMed] [Google Scholar]
  • 15.Smith AD, et al. Piezoresistive properties of suspended graphene membranes under uniaxial and biaxial strain in nanoelectromechanical pressure sensors. ACS Nano. 2016;10:9879–9886. doi: 10.1021/acsnano.6b02533. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 16.Patel RN, Mathew JP, Borah A, Deshmukh MM. Low tension graphene drums for electromechanical pressure sensing. 2D Mater. 2016;3:011003. [Google Scholar]
  • 17.Dolleman RJ, Davidovikj D, Cartamil-Bueno SJ, van der Zant HSJ, Steeneken PG. Graphene squeeze-film pressure sensors. Nano Lett. 2015;16:568–571. doi: 10.1021/acs.nanolett.5b04251. [DOI] [PubMed] [Google Scholar]
  • 18.Romijn, J. et al. A miniaturized low power pirani pressure sensor based on suspended graphene. in 2018 IEEE 13th Annual International Conference on Nano/Micro Engineered and Molecular Systems (NEMS) (IEEE, 2018).
  • 19.Rosłoń, I. E. et al. Graphene effusion-based gas sensor (2020). Preprint at https://arxiv.org/abs/2001.09509v1.
  • 20.Dolleman RJ, Cartamil-Bueno SJ, van der Zant HSJ, Steeneken PG. Graphene gas osmometers. 2D Mater. 2016;4:011002. [Google Scholar]
  • 21.Cartamil-Bueno SJ, et al. Very large scale characterization of graphene mechanical devices using a colorimetry technique. Nanoscale. 2017;9:7559–7564. doi: 10.1039/c7nr01766a. [DOI] [PubMed] [Google Scholar]
  • 22.Barton RA, et al. High, size-dependent quality factor in an array of graphene mechanical resonators. Nano Lett. 2011;11:1232–1236. doi: 10.1021/nl1042227. [DOI] [PubMed] [Google Scholar]
  • 23.Cartamil-Bueno SJ, et al. Colorimetry technique for scalable characterization of suspended graphene. Nano Lett. 2016;16:6792–6796. doi: 10.1021/acs.nanolett.6b02416. [DOI] [PubMed] [Google Scholar]
  • 24.Berger CN, Dirschka M, Vijayaraghavan A. Ultra-thin graphene–polymer heterostructure membranes. Nanoscale. 2016;8:17928–17939. doi: 10.1039/c6nr06316k. [DOI] [PubMed] [Google Scholar]
  • 25.Lin Y-C, et al. Graphene annealing: how clean can it be? Nano Lett. 2011;12:414–419. doi: 10.1021/nl203733r. [DOI] [PubMed] [Google Scholar]
  • 26.Ahn Y, Kim J, Ganorkar S, Kim Y-H, Kim S-I. Thermal annealing of graphene to remove polymer residues. Mater. Express. 2016;6:69–76. [Google Scholar]
  • 27.Huang L-W, et al. Characterization of the cleaning process on a transferred graphene. J. Vac. Sci. Technol. 2014;32:050601. [Google Scholar]
  • 28.Gammelgaard L, et al. Graphene transport properties upon exposure to PMMA processing and heat treatments. 2D Mater. 2014;1:035005. [Google Scholar]
  • 29.Jain A, et al. Minimizing residues and strain in 2D materials transferred from PDMS. Nanotechnology. 2018;29:265203. doi: 10.1088/1361-6528/aabd90. [DOI] [PubMed] [Google Scholar]
  • 30.Ruiz-Vargas CS, et al. Softened elastic response and unzipping in chemical vapor deposition graphene membranes. Nano Lett. 2011;11:2259–2263. doi: 10.1021/nl200429f. [DOI] [PubMed] [Google Scholar]
  • 31.Castellanos-Gomez A, et al. Elastic properties of freely suspended MoS2 nanosheets. Adv. Mater. 2012;24:772–775. doi: 10.1002/adma.201103965. [DOI] [PubMed] [Google Scholar]
  • 32.Nicholl RJ, et al. The effect of intrinsic crumpling on the mechanics of free-standing graphene. Nat. Commun. 2015;6:8789. doi: 10.1038/ncomms9789. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 33.Li Z, et al. Deformation of wrinkled graphene. ACS Nano. 2015;9:3917–3925. doi: 10.1021/nn507202c. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 34.Suk JW, Piner RD, An J, Ruoff RS. Mechanical properties of monolayer graphene oxide. ACS Nano. 2010;4:6557–6564. doi: 10.1021/nn101781v. [DOI] [PubMed] [Google Scholar]
  • 35.Gómez-Navarro C, Burghard M, Kern K. Elastic properties of chemically derived single graphene sheets. Nano Lett. 2008;8:2045–2049. doi: 10.1021/nl801384y. [DOI] [PubMed] [Google Scholar]
  • 36.Ferrari AC. Raman spectroscopy of graphene and graphite: Disorder, electron–phonon coupling, doping and nonadiabatic effects. Solid State Commun. 2007;143:47–57. [Google Scholar]
  • 37.Kim K, et al. Raman spectroscopy study of rotated double-layer graphene: Misorientation-angle dependence of electronic structure. Phys. Rev. Lett. 2012;108:246103. doi: 10.1103/PhysRevLett.108.246103. [DOI] [PubMed] [Google Scholar]
  • 38.Ni ZH, et al. Tunable stress and controlled thickness modification in graphene by annealing. ACS Nano. 2008;2:1033–1039. doi: 10.1021/nn800031m. [DOI] [PubMed] [Google Scholar]
  • 39.Eckmann A, et al. Probing the nature of defects in graphene by raman spectroscopy. Nano Lett. 2012;12:3925–3930. doi: 10.1021/nl300901a. [DOI] [PubMed] [Google Scholar]
  • 40.Šiškins M, et al. High-temperature electronic devices enabled by hBN-encapsulated graphene. Appl. Phys. Lett. 2019;114:123104. [Google Scholar]
  • 41.Son S-K, et al. Graphene hot-electron light bulb: incandescence from hBN-encapsulated graphene in air. 2D Mater. 2017;5:011006. [Google Scholar]
  • 42.Bunch, J. S. Mechanical and Electrical Properties of Graphene Sheets (Cornell University Ithaca, NY, 2008).
  • 43.Ponomarenko LA, et al. Density of states and zero landau level probed through capacitance of graphene. Phys. Rev. Lett. 2010;105:136801. doi: 10.1103/PhysRevLett.105.136801. [DOI] [PubMed] [Google Scholar]
  • 44.Xia J, Chen F, Li J, Tao N. Measurement of the quantum capacitance of graphene. Nat. Nanotechnol. 2009;4:505–509. doi: 10.1038/nnano.2009.177. [DOI] [PubMed] [Google Scholar]
  • 45.Harzheim A, Könemann F, Gotsmann B, van der Zant HSJ, Gehring P. Single-material graphene thermocouples. Adv. Funct. Mater. 2020;30:2000574. [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

41378_2020_212_MOESM1_ESM.docx (3MB, docx)

SUPPLEMENTARY INFORMATION: Sensitive capacitive pressure sensors based on graphene membrane arrays

Data Availability Statement

The manuscript has associated data in a data repository. The numerical data shown in figures of the manuscript can be downloaded from the Zenodo online repository at https://doi.org/10.5281/zenodo.4042077.


Articles from Microsystems & Nanoengineering are provided here courtesy of Nature Publishing Group

RESOURCES