Skip to main content
RSC Advances logoLink to RSC Advances
. 2026 Nov 17. Online ahead of print. doi: 10.1039/d6ra09329a

Copper-, nickel- and zinc-based trimetallic (CuNiZn–BDC) MOFs as efficient adsorbents for the adsorptive removal of metanil yellow from wastewater

Sultan Alam a, Ali Umar a, Muhammad Zahoor b,✉, Fatimah M Alzahrani c, Munawar Iqbal d,e
PMCID: PMC13776821  PMID: 43048204

Abstract

Herein, a trimetallic metal–organic framework was synthesized (abbreviated as TM-CuNiZn–BDC MOF) via a solvothermal method. The TM-CuNiZn–BDC MOF was comprehensively characterized by EDX, SEM, elemental mapping, XRD, FTIR spectroscopy, BET, zeta potential analysis, and TGA. FTIR spectroscopy confirmed the presence of key functional groups, while XRD revealed crystallinity with clear, sharp, and distinct diffraction peaks. TGA indicated stability up to 600 °C. The estimated surface area from BET analysis was 654 m2 g−1. The synthesized MOF exhibited a nanoscale size of approximately 98.3 nm with agglomerates of around 259 nm. Under optimal experimental conditions, such as 0.01 g adsorbent dosage, pH 6, 60 °C and 60 min contact time, the MOF achieved >93% removal efficiency for metanil yellow dye. Kinetic investigations revealed that the process followed second-order kinetics, as evidenced by the linear correlation (R2 = 0.99), while the adsorption capacity recorded was 689 mg g−1 at 333 K. The adsorption was spontaneous with a negative ΔG° value and endothermic with a positive ΔH°; the adsorption mechanism was governed by chemisorption, hydrogen bonding, electrostatic attraction, π–π interactions and pore filling. The TM-CuNiZn–BDC MOF retained its structural stability and 54% removal efficiency after seven reuse cycles, demonstrating its strong potential as a robust and efficient wastewater adsorbent.


Herein, a trimetallic metal–organic framework was synthesized (abbreviated as TM-CuNiZn–BDC MOF) via a solvothermal method.graphic file with name d6ra09329a-ga.webp

1. Introduction

Dyes are widely used in the leather, pharmaceutical, textile, healthcare, paper, and tannery industries, with the textile sector being the largest global consumer.1 It has been estimated that over 10 000 varieties of commercial dyes are in use today and that the world output has been over 7 × 105 metric tons. Among these dyes, the widespread use of metanil yellow, a synthetic mono-azo dye (C.I. acid yellow 36), across the textile, leather, shoe polish, paper, and even food industries, despite bans in many countries, has led to its pervasive discharge into water bodies, posing significant environmental and health hazards.2–4 It is documented to induce tumor-enhancing effects, testicular damage, altered DNA synthesis, hematological changes, methemoglobinemia, cyanosis, and allergic dermatitis upon exposure.5 Traditional treatment methods, such as coagulation, biological processes, photocatalytic degradation, and electrochemical oxidation, offer varying degrees of effectiveness; however, they often suffer from high operational costs, the formation of secondary pollutants, or limited selectivity toward stable dye molecules.6,7 Among these approaches, adsorption emerges as a versatile and efficient technique for dye elimination, offering simplicity in operation, high selectivity, and minimal sludge generation.8,9 A wide array of adsorbents, including activated carbon from sawdust or tree bark, bio-adsorbents like hen egg membranes, magnetic nanoparticle composites, hydrogels, zeolites, and graphene oxide, have been investigated, achieving capacities in the range of 100–130 mg g−1 and demonstrating moderate success in batch- or column-based systems.10,11 Nonetheless, these conventional materials often lack tunability and sustained performance under harsh wastewater conditions.12 The metal–organic frameworks, abbreviated as MOFs, are becoming popular, being highly efficient adsorbent materials with high surface areas (500 to 7000 m2 g−1), controllable pore structure, modifiable chemical functionalities, and robust surface interaction processes. Such interactions involve electrostatic attractions, hydrogen bonding, Lewis acid–base interactions and π–π stacking, which are all effective in increasing their affinity for a broad spectrum of adsorbates. Therefore, MOFs show much better adsorption activity than typical porous materials, like zeolites and activated carbons.13,14 While bimetallic MOFs already outperform their monometallic counterparts in terms of structural stability, porosity, active site availability, selectivity, and adsorption capacity, the shift toward trimetallic MOFs provides further synergistic benefits. These frameworks exhibit enhanced hierarchical porosity, improved mass transport, multiple binding environments, and increased robustness under variable pH or saline conditions.15 As an example, the Zn–Cu–Cr trimetallic MOF adsorbs Congo red at a very high adsorption affinity. This material showed good structural stability, whereby, after 72 h, it retained about 95% of its surface area, retained more than 90% dye removal capacity and power after five adsorption/desorption cycles, and had no leaching of metal ions (<1.2 ppm), having second-order kinetics and a Langmuir best fit of the data.16 Despite these successes, adsorption of metanil yellow using trimetallic MOFs remains largely unexplored. Considering the dye's ionic nature, chemical stability, and toxicity profile, there is a compelling need to develop a continuous-flow adsorption system using a trimetallic MOF as the active adsorbent.

This study focuses on the synthesis of a highly efficient, porous TM-CuNiZn–BDC MOF tailored for metanil yellow removal, and the comprehensive evaluation of its structural characteristics, adsorption kinetics and isotherms, and reusability performance.

The CuNiZn trimetallic composition was selected to exploit the synergistic effects of the constituent metal ions. The Cu2+ ions form stable MOF structures due to their high coordinating strength, Ni2+ ions provide extra active sites and further adsorption interactions, and Zn2+ ions allow for a more stable structure and increased porosity. These metals in the same framework are likely to combine to yield improved surface properties, a variety of active sites, and better adsorption capabilities than monometallic MOFs.

We aim to demonstrate that this adsorbent not only offers superior adsorption capacity and removal efficiency but also maintains structural stability in realistic wastewater conditions, thereby presenting a viable pathway for scalable, sustainable dye elimination.

2. Experimental design

2.1. Reagents

Copper(ii) nitrate [Cu(NO3)2·6H2O] ≥99.99%, nickel nitrate [Ni(NO3)2·6H2O] ≥99.0%, zinc nitrate [Zn (NO3)2·6H2O] ≥99.0%, ethanol ≥99.8%, sodium hydroxide (NaOH) ≥99.99%, benzene-1,4-dicarboxylic acid ≥98.6%, DMF ≥99.8%, HNO3 ≥99.99%, sodium nitrate NaNO3 ≥99.99%, acetone ≥99% and metanil yellow dye (MY) ≥98.99% reagents were obtained from Sigma-Aldrich and were directly utilized with no further purification. Table 1 presents the physicochemical characteristics of metanil yellow dye, and Fig. S1 shows its physical appearance and chemical structure.

Table 1. Characteristics of metanil yellow dye.

Chemical formula C18H15N3NaO3S
IUPAC name Sodium 3-[(4-anilinophenyl)diazenyl]benzenesulfonate
Molecular mass 376.39 amu
Maximum wavelength 434 nm
% purity ≥98%
Solubility Highly soluble in water
CAS number 587-98-04
Physical appearance Yellow-orange powder
Class Anionic azo dye

2.2. TM-CuNiZn–BDC MOF synthesis

Trimetallic CuNiZn–BDC was synthesized via a conventional solvothermal method in a Teflon-lined stainless-steel autoclave reactor (Fig. S2). Copper nitrate (Cu(NO3)2), nickel nitrate (Ni(NO3)2), zinc nitrate (Zn(NO3)2) and terephthalic acid (H2BDC) were used without any further purification. First, 2.174 g of Cu(NO3)2 (≈9 mmol), 2.617 g of (Ni(NO3)2) (≈9 mmol), 2.678 g of (Zn(NO3)2) (≈9 mmol), and 1.240 g of H2BDC (BDC) (≈7.5 mmol) were dissolved in 500 mL of DMF to ensure complete solubilization; a homogeneous blue solution was obtained, which was stirred at a temperature of 70 °C for 1 hour.17 The precursor solution was transferred into a Teflon-lined autoclave vessel, which was sealed and placed in a convection oven. The assembly was heated at 160 °C for 48 h under autogenous pressure. Upon completion, the autoclave was allowed to cool naturally to room temperature. A blue crystalline precipitate was formed, which was recovered by centrifugation at 5000 rpm. The MOF powder was washed three times with DMF to remove unreacted ligands and solvated impurities, followed by three washes with ethanol to displace residual DMF and gently activate the pore structure. Finally, the MOF was dried under vacuum at 60–80 °C for 8 h to ensure the removal of guest molecules and activation of porosity.18

2.3. Standard curve

A standard curve (calibration curve) for metanil yellow (MY) was established through the preparation of multiple standard solutions at varying concentrations (10–60 mg L−1), derived from a stock solution, and their absorbance was analyzed at λmax = 434 nm. The correlation coefficient (R2 ≈ 1) confirmed the linearity (Fig. S3). A trend line equation [y = mx + C] was used for the analysis of the unknown concentration of the samples (Table 2).

Table 2. Calculated parameters for the adsorption kinetics of metanil yellow onto the TM-CuNiZn–BDC MOF.

Parameter 293 K 313 K 333 K
Pseudo-first-order kinetic model
q e,exp (mg g−1) 184.6 194.5 198.2
k 1 (min−1) 0.033 0.034 0.048
q e,cal (mg g−1) 24.03 28.2 48.39
 
Pseudo-second-order kinetic model
q e,exp (mg g−1) 184.6 194.5 198.2
k 2 (min−1) 0.0019 0.0096 0.015
q e,cal (mg g−1) 171.31 183.31 196.31
 
Comparison of the statistical parameters of pseudo 1st- and pseudo 2nd-order models
1st order 2nd order 1st order 2nd order 1st order 2nd order
R 2 0.932 0.996 0.921 0.999 0.934 0.998
χ 2 139.7 0.322 142.2 0.1555 113.2 0.1744
SEE 25 782 160.6 27 655 166.3 22 443 149.8
RMSE 160.6 7.71 166.3 5.5 149.8 5.88
 
Intraparticle diffusion model
k id (mg g−1 min−1/2) 3.088 4.229 6.333
C 175.34 161.04 136.5
R 2 0.98 0.981 0.987
 
Boyd's film-diffusion model
Slope (m) 0.0572 0.0484 0.0486
Intercept (C) 0.689 1.361 1.672
R 2 0.984 0.991 0.997
 
Power function model
a 123.88 151.71 167.11
b 0.042 0.059 0.097
R 2 0.998 0.973 0.998
 
Elovich model
α 202.29 1034.31 9632.87
β 0.061 0.093 0.126
R 2 0.998 0.973 0.998

2.4. Instrumentation

The synthesized CuNiZn–BDC MOF was characterized using a suite of analytical instruments to evaluate the morphology, structure, surface properties, thermal stability, and elemental composition. Scanning Electron Microscopy (SEM) (JSM-5910, Japan) was utilized for morphological analysis, at accelerating voltages typically between 2–30 kV, with a maximum magnification of 300 000× and a resolution of 2.3 nm. The FTIR spectrum was taken in KBr pellet mode at (4000–400 cm−1) using a Cary 630 FTIR spectrophotometer (Agilent, Canada). N2 adsorption–desorption analysis was conducted using the BET and BJH techniques for the determination of specific surface area; the measurements were performed at 77 K. Before testing, all samples were vacuum-degassed overnight at 110 °C to eliminate physically adsorbed species. Thermogravimetric analysis was utilized to determine the thermal robustness of the MOF, increasing the temperature from 25 °C to 700 °C. Zeta potential analysis was conducted with a dynamic light scattering (DLS) instrument (Zeta-sizer Blue, from Malvern PANalytical UK) to assess surface charge and colloidal stability. Elemental mapping and compositional analysis were conducted using EDX detectors integrated with the SEM system at ∼20 kV, revealing the spatial elemental distribution across MOF crystals.

2.5. Sorption experiments

The stock solution of the selected dye was prepared using deionized water at a concentration of about 1000 ppm and was subsequently used for the investigation of the adsorption kinetics, the characteristics of the equilibria, the mechanism, and the impact of major operational parameters. In each batch experiment, 0.01 g of the TM-CuNiZn–BDC MOF was introduced into 0.01 L of MY solution of known concentration in flasks. The adsorbent–adsorbate solution was stirred at 150 rpm using a water-bath shaker for specific intervals of time. At each sampling point, an aliquot was taken out, filtered, and its residual dye concentration (final dye concentration) evaluated at the wavelength of maximum absorbance (λmax = 434 nm) using a UV-visible spectrophotometer. From these data, the adsorptive removal efficiency (% R), as well as adsorption capacity (qt), were subsequently determined.

2.6. Effects of different operational parameters

To analyze the effect of time on the adsorptive elimination of the MY dye and determine the equilibrium time, 0.01 g of adsorbent (TM-CuNiZn–BDC MOF) was introduced into 10 mL of 200–400 mg per L dye solution in reagent bottles. The mixtures were agitated at room temperature for 30 to 180 minutes. Samples were taken out at regular intervals, followed by filtration, and analysis using UV-visible spectrophotometry at λmax = 434 nm (for the dye) to monitor residual concentrations.

To optimize the dosage of the adsorbent, the quantity of adsorbent was varied (between 0.005 and 0.03 g) with all other parameters being set at the same levels (volume, 10 mL; initial concentration of dye, 200 ppm; pH, 6; 60 minutes; 25 °C). The suspensions were filtered and the absorbance was measured using a UV-visible spectrophotometer to determine the concentration of metanil yellow that remained. Percentage removal was then determined for each dose of adsorbent. The pH was adjusted using 0.1 M NaOH or HCl and measured at the start of adsorption while keeping other parameters constant. Temperature effects were evaluated at 283, 293, 303, 313, 323, and 333 K under identical conditions. Once equilibrium was attained, the concentration of metanil yellow left in the solution was calculated.

The impact of the initial dye concentration was investigated by varying it from 50 to 250 mg L−1, with all other parameters kept fixed. Adsorption capacity and percentage removal % R were computed using expressions (1) and (2). The amount of dye that was still present in the filtrate after each experiment was analyzed using UV-visible spectrophotometry at λmax = 434 nm.

2.7. Adsorption performance

Eqn (1) was used to calculate percentage removal % R, and eqn (2) was used for the calculation of adsorption capacity, qt as follows:

2.7. 1
2.7. 2

In the above equations, C0, Ct, W, and V denote the adsorbate concentration (before adsorption), concentration of residual dye at a given time t, mass of adsorbent and solution volume of dye, respectively.

2.8. Replication of adsorption experiments

For ensuring reproducibility, some experiments were conducted in triplicate, maintaining an error threshold within 5%. Mean values of all three independent trials have been presented in Table 3. Kinetic model fitting (PFO and PSO) was performed by non-linear regression using the Excel Solver add-in, followed by error analysis based on χ2, SSE, and RMSE.19 The chi-square statistic was calculated as follows:

2.8. 3
2.8. 4
2.8. 5

Table 3. Adsorption isotherm study parameters for the adsorptive elimination of metanil yellow on the TM-CuNiZn–BDC MOF.

Parameter 293 K 313 K 333 K
Langmuir isotherm model
Q m (mg g−1) 588.2 625 689.7
K L 0.018 0.029 0.038
R L 0.100 0.065 0.056
R 2 0.995 0.995 0.996
 
Freundlich isotherm model
K F (mg g−1) 19.058 28.571 38.642
n 1.493 1.526 1.607
R 2 0.912 0.915 0.923
 
Temkin isotherm model
K T 0.237 0.391 0.567
B 113.6 116.7 118.6
β (J mol−1) 21.45 21.95 23.72
R 2 0.977 0.968 0.973
 
Dubinin–Radushkevich (D–R) isotherm model
q D–R (mg g−1) 255.19 266.67 280.33
γ (mol2 kJ−2) 0.0079 0.0057 0.0019
E (kJ mol−1) 7.955 9.365 16.22
R 2 0.713 0.752 0.753

2.9. Adsorption kinetics and isotherm studies

Kinetics and equilibrium isotherms were investigated for metanil yellow MY adsorption on the TM-CuNiZn–BDC MOF. Kinetic experiments (0.01 g in 10 mL of 200 mg per L MY, pH 6, 293–333 K, 150 rpm) followed the uptake of dye within 10–60 min and were fitted to various kinetic models to determine rate constants and rate-limiting steps. In the adsorption isotherm experiments, the MY dye concentration was varied from 50 to 500 mg L−1 at temperatures ranging from 293 to 333 K and a contact time of 60 minutes to determine the equilibrium adsorption capacity (qe). The Freundlich, Langmuir, Temkin and Dubinin–Radushkevich isotherm models were utilized for the determination of adsorption capacity, surface heterogeneity, and adsorption mechanism. Combined, these studies gave a clear picture of the kinetic and thermodynamic characteristics of the MOF–MY dye adsorption process.

2.9. 6

2.10. Recyclability of CuNiZn–BDC MOF

To investigate the regeneration efficiency and recyclability of the TM-CuNiZn–BDC and reuse for metanil yellow dye removal, adsorption–desorption cycles were systematically performed. After a typical adsorption run, the dye-saturated MOF MY@CuNiZn–BDC was recovered via centrifugation and treated with a mixture of ethanol, acetone, and sodium hydroxide under stirring for approximately 60 minutes to strip the dye from the adsorbent's active sites.19 The adsorbent was then carefully rinsed with distilled water to eliminate all traces of dye, dried at 70 °C for 7 hours and reused in successive adsorption cycles.

3. Results and discussion

3.1. Surface point of zero charge (pHpzc) analysis

The point of zero charge (pHpzc) is the pH at which a material's surface, such as trimetallic CuNiZn–BDC, has no net electrical charge, meaning it has an equal number of H+ and OH− ions; it is a crucial parameter for understanding and controlling surface interactions during adsorption. pHpzc was experimentally measured using the drift method. In this process, a series of 20 mL tubes were used to disperse 0.1 g of CuNiZn–BDC MOF in 10 mL of 0.1 M NaNO3 solution. The initial pH of the solutions was adjusted across a range (pH 2–12) using 0.1 M NaOH and 0.1 M HNO3 solutions, equilibrated for 24 h with agitation in a water bath shaker at 150 rpm; after this process, the final pH (pHf) was measured.20 By plotting ΔpH (pHf − pHi) versus pHi, the pHpzc was determined at the point where ΔpH = 0, corresponding to a value of 7.45, as shown in Fig. S5. pH below this value indicates a positively charged surface, while a higher value than this indicates a negatively charged surface, which guides adsorption behavior and the optimization of dye removal conditions. According to previous studies, the pHpzc of related MOF-based adsorbents was reported between ∼3.9 and ∼7.8, depending on surface functionalization and the metal center.21 As a result, the adsorption performance across different ionic species can be fine-tuned by adjusting the working pH relative to the pHpzc; at or near neutrality, where electrostatic forces diminish, more specific mechanisms, such as chelation, surface complexation, or ion exchange, can dominate.

3.2. Characterization of trimetallic CuNiZn–BDC MOF

3.2.1. Scanning electron microscopy (SEM)

Micrographs of the trimetallic CuNiZn–BDC MOF revealed a hierarchical agglomerated morphology consisting of irregular plate-like and cubic microcrystals that range from sub-micron to a few microns in size, indicative of the co-integration of multiple metal centers influencing crystal growth and assembly (Fig. 1). Low-magnification micrographs showed loosely packed micron-scale clusters, while high-resolution images revealed well-defined, faceted cubic and plate-like crystallites with textured, rough surfaces, features that point to interconnected porosity and high surface roughness that are favorable for adsorbate uptake. A histogram analysis confirmed an average agglomerate size of around 259 nm (by the average grain intersection (AGI) method), indicating a nanoscale aggregation regime that maintains excellent accessibility and diffusion dynamics crucial for adsorption processes. The same morphological pattern has also been reported in other trimetallic MOFs, where the co-integration of multiple metal centers induces analogous clustered crystal habits.

Fig. 1. SEM micrographs acquired at (a) 2500× and (b) 30 000× magnification. (c) Particle size distribution histogram.

Fig. 1

3.2.2. Energy-dispersive X-ray spectroscopy (EDX)

EDX analysis of the TM-CuNiZn–BDC MOF confirmed the presence of all the constituent elements, like oxygen, carbon, copper, nickel, and zinc, with no significant impurities, and, consequently, a successful synthesis. Carbon (C) and oxygen (O), which constitute the dominant backbone linker system, account for approximately 61.2 mass%. Although the synthesis of the TM-CuNiZn–BDC MOF was performed using equimolar quantities of the precursor salts of Cu, Ni and Zn, the corresponding metal weight percentages from the EDX analysis were found to be 13.20%, 12.40%, and 12.10%, respectively, giving an approximate relative molar ratio of Cu : Ni : Zn = 1.14 : 1.12 : 1.00, which means a near-equimolar distribution of the three metals in the synthesized MOF. The fact that the mass percentages of the three metals are similar suggests that the composition of the MOF structure is trimetallic, and not surface enrichment. However, the presence of N in the EDX analysis may be attributed to residual DMF molecules or traces of nitrate precursors remaining after the synthesis process. The EDX spectrum (Fig. 2) and element mapping (Fig. S6) confirmed the presence of Ni, Cu, and Zn in the CuNiZn–BDC MOF. Further, the SEM-EDX elemental mapping revealed the homogeneous co-integration of the constituent elements throughout the CuNiZn–BDC MOF, which has also been reported for trimetallic MOFs, including FeCoNi–BDC; the elemental maps revealed uniform distribution of metal centers in the crystals.22

Fig. 2. Elemental composition and EDX spectrum of trimetallic CuNiZn–BDC MOF.

Fig. 2

3.2.3. FTIR spectroscopic analysis

The FTIR spectrum for TM-CuNiZn–BDC MOF confirmed the successful complexation between metal nodes and the BDC linker through several distinctive vibrational features. The broad absorption peak at 3200–3600 cm−1 is correlated to O–H bond stretching vibrations, indicative of the surface-bound water molecules and residual (uncoordinated) –COOH groups. This feature enhances the hydrophilicity of the material and facilitates stronger interactions with aqueous dye molecules.23 The band observed between 1500 cm−1 corresponds to aromatic C Created by potrace 1.16, written by Peter Selinger 2001-2019 C stretching, corroborating the presence of benzene rings in the structure of the linker, which may facilitate π–π stacking during the metanil yellow dye adsorption. Simultaneously, the sharp peak at 1650 cm−1 indicates carbonyl stretching of coordinated carboxylate groups, which proves the successful formation of coordinate covalent bonds between metal ions and the BDC ligand (Fig. 3a). Weaker signals around 1025 and 730 cm−1 correspond to C–H bending (aromatic) and deformations in the ring, which indicate the structural features of the linker (benzene-1,4-dicarboxylate). Moreover, peaks lower than 1000 cm−1, between 400–800 cm−1, correspond to M–O–C and M–O bonds, which support the fact that chelation is strong in the cluster of the MOF.17 All these spectral features are clear indications that a trimetallic coordination network has been formed successfully with metal–oxygen coordination bonds, with intact and fully incorporated organic linkers. The MOF surface enables multiple adsorption pathways for metanil yellow, including metal–dye coordination, π–π stacking, electrostatic attraction to positively charged sites and hydrogen bonding. All these interactions have a synergistic effect on the efficient adsorption of metanil yellow.

Fig. 3. (a) FTIR spectrum and (b) thermogram of the TM-CuNiZn–BDC MOF.

Fig. 3

3.2.4. Thermogravimetric analysis (TGA)

The thermal behavior of the trimetallic CuNiZn–BDC MOF was examined by thermogravimetric analysis (TGA) under a continuous flow of N2 (30 mL min−1) in the temperature range of 30–700 °C (Fig. 3b). The thermogram shows three different phases of weight loss. The first stage (below about 200 °C) represents the loss of about 30% of the sample weight, mainly due to the evaporation of the adsorbed water, residual DMF and other solvent molecules.24 The second stage, which occurs between ∼200 °C and ∼450 °C, corresponds to additional weight loss resulting from the BDC organic linker decomposition and the gradual loss of the MOF coordination network.25 At temperatures higher than about 450 °C, a further loss in weight occurs, possibly due to further decomposition of organic species remaining and/or transformation of the metal-containing framework into more thermally stable inorganic species. The solid residue has been shown to probably be a mixture of CuO, NiO and ZnO, but other complementary phase characterization methods would be required to verify the identities. These results show the temperature dependence of the thermal stability of CuNiZn–BDC. The material loses a significant amount of solvent and the framework decomposes at high temperatures, but the inorganic skeleton has higher thermal stability. The results of the TGA therefore do not indicate that the intact MOF framework is stable up to 600 °C, but rather that there is a progressive degradation of the MOF structure, which is followed by the creation of a more thermally stable residue. The potential for use in high-temperature water-treatment applications should therefore be evaluated based on the specific operating temperature and the stability of the material under the conditions of water treatment.26

3.2.5. Brunauer–Emmett–Teller (BET) analysis

Fig. 4 shows a BET plot of the TM-CuNiZn–BDC MOF, which reflects a type 1 isotherm and indicates that the material has a microporous structure and is characterized by well-defined porosity and a highly accessible internal surface. The BET specific surface area was determined to be 654 m2 g−1, while the Langmuir surface area was about 671 m2 g−1; these findings are in close agreement, which supports the reliability of the surface area determinations. Such elevated surface area values indicate the presence of an extensive internal porous network and show a high degree of suitability for adsorption operations.27 A well-developed microporous framework is suggested by the BET average pore diameter of 19.68 Å (1.938 nm), while a substantial mesoporous regime is confirmed by the BJH-derived average diameter of 36.845 Å (3.685 nm). The total pore volume of the material determined was about 0.03474 cm3.

Fig. 4. N2 adsorption–desorption plots of TM-CuNiZn–BDC MOF.

Fig. 4

3.2.6. Zeta potential analysis

The zeta potential of trimetallic CuNiZn–BDC MOF is graphically presented in Fig. S9, revealing that the synthesized TM-CuNiZn–BDC has a slightly negative zeta potential (−11 mV), which could be explained by the deprotonated hydroxyl (OH−) and carboxyl (COO−) functional groups, leading to moderate colloidal stability. A narrow zeta dispersion (2.60 mV) validates the presence of uniformity in surface charge and enhances uniform dye adsorption.28 The low conductivity of 0.0473 mS cm−1 (ref. 28) indicates a low ionic strength, which may influence attractive electrostatic interactions between the MY dye and TM-CuNiZn–BDC MOF. Nevertheless, the adsorption capacity can be greatly elevated by controlling the pH of the adsorption system because the pH determines the extent of H+ binding with surface –COO− and OH− functional groups. This kind of modulation of the charge on the surface allows one to optimize electrostatic attractive interactions between the synthesized MOF and dye molecules, resulting in an improved adsorption performance.

3.2.7. X-ray diffraction (XRD) studies

XRD analysis was performed to evaluate the purity of the sample's phase, crystallite size, structural integrity and crystallinity. As demonstrated in Fig. 5, the diffraction pattern has discrete characteristic peaks at 2θ = 39.5°, 29.3°, 25.9°, 24.1°, 20.2°, 19.0°, 15.6°, 13.8°, 12.9° and 11.3°, which are similar to the previous bimetallic CuZn–BDC MOF studies. This matching of peak positions confirms that the desired framework has been successfully constructed and well preserved.29 However, the presence of additional diffraction peaks at 15.8°, 16.8°, and 20.7°, which correspond to those found in the Ni–BDC MOF, implies that Ni2+ has been successfully integrated into the framework structure.30 Using the FWHM data and the Scherrer equation, the average crystalline size of the particles was determined to be 98.3 nm.31 Crystallinity (%) was estimated from the XRD pattern, which was 72.7%. Distinct, sharp diffraction peaks indicate that the synthesized MOF has moderate, yet appreciable crystallinity.32

Fig. 5. XRD spectrum of the TM-CuNiZn–BDC MOF.

Fig. 5

3.3. Effects of varying experimental conditions on the adsorption of metanil yellow onto the TM-CuNiZn–BDC MOF

3.3.1. Effect of contact time

The impact of contact time on the adsorption performance of the TM-CuNiZn–BDC MOF on metanil yellow (MY) was explored with initial dye concentrations of 200 to 400 mg L−1 over contact times of 30–180 minutes. Fig. 6a reveals that the MOF undergoes a fast initial uptake followed by the gradual achievement of equilibrium. The adsorption capacity increases sharply within the first 30 to 60 minutes, which is likely due to the availability of abundant active sites and a strong concentration gradient. As the available external surface-active sites on the TM-CuNiZn–BDC MOF adsorbent become saturated, the adsorption rate decreases as intraparticle diffusion becomes the controlling step.33 During that interval (60–120 min), equilibrium is established, and beyond this, there is a negligible rise in the adsorption capacity (qt). The transport of MY dye into the interior pores becomes the rate-determining step at this stage. Eventually, the system achieves equilibrium.

Fig. 6. Effects of operational parameters on the adsorption of the metanil yellow dye on trimetallic CuNiZn–BDC MOF: (a) contact time, (b) pH, (c) temperature, (d) adsorbent dosage and (e) concentration.

Fig. 6

3.3.2. Effect of pH

As metanil yellow is a negatively charged azo dye, its adsorption greatly depends on the medium's pH. The adsorption efficiency with varying pH was examined using a concentration of 200 mg L−1 in the pH range of 2 to 12, as shown in Fig. 6b. It was found that, under strongly acidic conditions, such as pH 2–4, the CuNiZn–BDC MOF adsorbent surface becomes protonated and the positively charged surface fosters strong attraction towards the negatively charged metanil yellow dye, yielding maximum dye uptake (≥93%). As the pH increased to the pHpzc value (7.45) of the adsorbent, there was a slight decrease in adsorption efficiency as the surface of the MOF became neutral and electrostatic interactions diminished. In contrast, an increase in pH above the pHpzc led to deprotonation, charge reversal, electrostatic repulsion, and competition of the anionic dye with OH− ions, significantly reducing the adsorption efficiency (54% at pH 12). Although the maximum adsorption efficiency was observed under strongly acidic conditions (pH 2–4), pH 6 was selected for subsequent adsorption experiments due to its near-neutral condition, which ensures better structural stability of the MOF and minimizes the possibility of framework degradation and metal ion leaching in highly acidic media. Furthermore, the adsorption efficiency at pH 6 was sufficiently high; therefore, pH 6 was a more practical and relevant operating condition for real wastewater treatment.34

3.3.3. Effect of temperature

The adsorption of metanil yellow onto the TM-CuNiZn–BDC MOF demonstrates a temperature-dependent and endothermic nature. The study was carried out using 200 mg per L dye at varying temperatures. It was found that the efficiency progressively increased from 78% at 283 K to 96% at 333 K (Fig. 6c). At lower temperatures, the dye uptake was limited due to reduced molecular diffusion and collision, and weak adsorbate–adsorbent interactions, while higher temperatures enhance the molecular mobility, pore expansion, and intraparticle diffusion, as they collectively overcome activation energy barriers and strengthen the MY–CuNiZn–BDC MOF interactions.35 The endothermic nature of the present study can be further substantiated through thermodynamic parameters (positive enthalpy change and spontaneous entropy change).

3.3.4. Effect of adsorbent dosage

Surface accessibility, active site density, and functional group chemistry strongly influence the TM-CuNiZn–BDC MOF's adsorption efficiency. The effect was investigated using 200 mg per L dye concentration and varying the adsorbent dose. Fig. 6d illustrates the impact of the adsorbent CuNiZn–BDC MOF amount on the % efficiency of metanil yellow dye, which shows a rapid rise in the adsorption followed by a plateau. The same pattern was observed in the literature.36 The identified trend of increasing removal efficiency as the dose of adsorbent increases is attributable to more active sites being accessible for dye uptake. The study revealed an increase in removal efficiency from 74% at 0.005 g to 91% at 0.025 g, followed by a plateau indicating a threshold dosage, above which further addition does not give an appreciable yield due to agglomeration and the resulting reduction in the accessible surface area.

3.3.5. Concentration effect

The adsorption process was assessed across the dye concentration range of 50–250 mg L−1, as shown in Fig. 6e. The figure demonstrates that the increase in the initial MY dye concentration leads to a reduction in the percentage adsorption efficiency, highlighting the interplay between the concentration gradient and surface coverage. At lower concentrations, the strong concentration gradient enables nearly complete utilization of available active sites, resulting in the maximum removal percentage. However, as the concentration of the dye rises, the finite active sites eventually reach saturation, causing a decline in the relative percentage removal.37 Therefore, 200 mg L−1 was chosen to be the optimal initial dye concentration, offering an ideal balance between superior adsorption capacities and real-world applicability.

3.4. Kinetic study

3.4.1. Pseudo-first- and pseudo-second-order kinetic models

Pseudo-first- and pseudo-second-order models were applied to determine the rate-limiting mechanism of metanil yellow adsorption on the TM-CuNiZn–BDC MOF,38 as shown in Fig. 7. The pseudo-first-order model, which is usually used to explain physisorption at active sites, is given as follows:

ln(qe − qt) = ln qe − k1/2.303. 7

Here, qt and qe are the adsorbent capacities at time t and at equilibrium, respectively, and k1 is the pseudo-first-order rate constant. In this system, the large difference between qe(cal) and qe(exp) and the low coefficient of regression showed that this model did not provide sufficient information on the adsorption kinetics (Table 3). Conversely, the pseudo-second-order model is mathematically given as follows:

t/qt = 1/k2qe2 + t/qe. 8

Here, k2 is the pseudo-second-order rate constant. Table 3 shows that the calculated (qe,cal) and experimental (qe,exp) equilibrium adsorption capacities of MY closely agree. The data exhibited a high correlation value (R2 ≥ 0.99), which strongly suggests that ion exchange governs the process and is an indication of surface-controlled chemisorption.39 Additionally, the rate constant k2 and qe(cal) values increase with temperature, indicating endothermic, temperature-dependent adsorption.

Fig. 7. Kinetic behavior of the metanil yellow dye on trimetallic CuNiZn–BDC MOF: (a) pseudo-1st-order kinetic model and (b) pseudo-2nd-order kinetic model.

Fig. 7

3.4.2. Weber–Morris intra-particle and Boyd diffusion models

The Weber–Morris intra-particle diffusion model can be mathematically expressed as follows:

3.4.2. 9

The diffusion mechanism of metanil yellow (MY) adsorption on the TM-CuNiZn–BDC MOF was examined using diffusion mechanism analysis models. The Weber–Morris model (eqn (9)) was used in the evaluation of the contribution of intraparticle diffusion. kid represents the rate of intraparticle diffusion, and C represents the thickness of the boundary layer.40 The resulting qtvs. t1/2 (Fig. 8a) plots show multilinearity with non-zero intercepts (Table 3), which suggests that adsorption occurs in a combination of several stages, such as rapid film diffusion and intraparticle diffusion, and intraparticle diffusion does not control the adsorption rate. Further insights into the controlling mechanism were gained using the Boyd model (eqn (10)) as follows:

3.4.2. 10
Fig. 8. Diffusion model analysis of the adsorption of metanil yellow on trimetallic CuNiZn–BDC MOF: (a) intraparticle diffusion and (b) Boyd diffusion.

Fig. 8

The Boyd plots (Fig. 8b) revealed that the behavior is linear with non-zero intercepts and high correlation coefficients (Table 3), which indicates that the overall adsorption rate is mainly controlled by film diffusion. Overall, the results indicate that MY adsorption on the TM-CuNiZn–BDC MOF is governed by both film diffusion and intraparticle diffusion, with the former being dominant. These findings suggest that film diffusion controls mass transfer rather than intraparticle diffusion. The same trend aligns with the previous studies for the adsorption of methylene in MIL-101(Fe).41

3.4.3. Elovich model

This model was employed for further explanation of 2nd order kinetics, under the supposition that the adsorbent surface has heterogeneous energy sites. Mathematically, this model is expressed as follows:

3.4.3. 11

where α is the chemisorption rate constant (mg g−1 min−1), and β represents the desorption constant (g mg−1). A larger value of α represents a faster initial rate of adsorption, while β is related to the extent of surface coverage and the amount of energy required for desorption. These parameters can be calculated from the slope and intercept of the plot of qtvs. ln(t) (Fig. 9a), and their values are listed in Table 3. The findings show that the desorption constant β increases with rising temperature, indicating a stronger interaction between the dye and the CuNiZn–BDC MOF adsorbent as the temperature rises. The rate constant α also increases with increasing temperature, suggesting that the process becomes more favorable as the temperature rises.42

Fig. 9. (a) Elovich and (b) power function models for the adsorptive removal of metanil yellow dye on trimetallic CuNiZn–BDC MOF.

Fig. 9

3.4.4. Power function model

This model can be mathematically presented as follows:

ln qt = ln a + b ln t. 12

In the equation above, the rate constant for initial adsorption is a, while b is the time-dependent rate constant; this model describes adsorption where the rate decreases over time, and the results are depicted by the slope and intercept of the ln qtvs. ln t plot. Fig. 9b can be used for obtaining the value of these constants, as presented in Table 3. The value close to 1 indicates a relatively steady adsorption rate. A lower value of b shows that there is a marked slowing as the surface-active sites have decreased accessibility.43 As temperature increases, the initial adsorption rate constant, a, in the power function model increases, indicating an improvement in initial adsorption efficiency, while the rate of adsorption decreases more slowly over time, as indicated by the rising time dependency constant b. In the case of metanil yellow adsorption onto CuNiZn–BDC MOF, the increase in a as well as b with increasing temperature indicates an enhancement in the efficiency of initial adsorption and a slower decline in adsorption rate at higher temperatures.

3.5. Adsorption isotherm study

Adsorption isotherm data were fitted to Langmuir, D–R, Freundlich and Temkin isotherm models to reveal essential adsorption properties such as maximum adsorption capacity, surface heterogeneity, interaction strength, and adsorption nature.

3.5.1. Langmuir isotherm model

According to this model, adsorption occurs as a monolayer over a homogeneous surface having identical, non-interacting sites and is given by the following equation:

3.5.1. 13

Here, Ce (mg L−1) is the equilibrium dye concentration, qe (mg g−1) is the adsorption capacity at equilibrium, Qm (mg g−1) is the maximum monolayer capacity, and KL (L mg−1) represents the adsorbate–adsorbent affinity. The parameters are determined from the slope and intercept of the Ce/qevs. Ce plot (Fig. 10a) as follows:

3.5.1. 14

In eqn (14), C0 denotes the initial concentration of the dye, KL refers to the Langmuir affinity constant, whose value determines the viability of the adsorption, and RL indicates adsorption behavior: a 0 value of RL denotes irreversible adsorption, while (0 < RL < 1) shows favorability of the adsorption, and RL = 1 represents the unfavorable nature of the process.44Table 4 contains the values of all these variables.45 In our study, Qm increased with temperature, highlighting its endothermic adsorption behavior. Meanwhile, RL values fall between 0 and 1 across these temperatures, reflecting consistently favorable adsorption conditions. The maximum adsorption capacity of 689.7 mg g−1 at 333 K was estimated from this model and represents a model-derived parameter rather than an experimentally measured uptake; therefore, it should be interpreted in light of the experimental concentration range and the goodness of fit.

Fig. 10. (a) Langmuir and (b) Freundlich isotherm models for the adsorption of the metanil yellow dye on trimetallic CuNiZn–BDC MOF.

Fig. 10

Table 4. Nonlinear regression parameters and statistical goodness-of-fit metrics for the isotherm models.
Temperature (K) Isotherm model R 2 RMSE RSS AIC
293 K Langmuir 0.9981 4.903 240.35 35.80
Freundlich 0.9897 11.273 1270.7 52.45
Temkin 0.9744 17.776 3159.8 61.56
D–R 0.8609 41.423 17 158.5 78.48
313 K Langmuir 0.9990 3.820 145.95 30.81
Freundlich 0.9859 14.436 2083.9 57.39
Temkin 0.9680 21.700 4709.03 65.55
D–R 0.8802 42.009 17 647.4 78.76
333 K Langmuir 0.9942 9.560 913.97 49.15
Freundlich 0.9865 14.551 2117.3 57.55
Temkin 0.9777 18.695 3495.07 62.57
D–R 0.8577 47.255 22 330.1 81.11

3.5.2. Freundlich isotherm model

This model serves as an experimental approach used to explain adsorption onto energetically heterogeneous surfaces and the possibility of multilayer uptake. Its linear form is as follows:

3.5.2. 15

where KF (mg g−1) corresponds to the Freundlich adsorption capacity constant and n is a dimensionless quantity that indicates the adsorption favorability.

For a plot of ln qevs. Ce, the intercept yields the KF value, while the slope gives the n value (Fig. 10b). In general, (1 < n < 10) indicates favorable adsorption and increasing surface heterogeneity. In our study, the value of KF increases with temperature, resulting in enhanced adsorption capacity at higher temperatures.45 Additionally, the n values of approximately across temperatures indicate favorable adsorption and moderate surface heterogeneity, consistent with typical dye-adsorbent systems.46

3.5.3. Temkin isotherm model

The Temkin model is suitable for systems in which chemisorption occurs, and the adsorption energy distribution across the binding sites exhibits a peak corresponding to the maximum adsorption energy and a linear decrease in heat of adsorption as the surface is covered. It can be expressed as follows:

qe = β ln KT + β ln Ce. 16

Here, in the equation above, KT (L mg−1) denotes the Temkin equilibrium binding constant reflecting interaction strength, and β (J mol−1) is associated with the adsorption heat.47 By plotting qevs. ln Ce (Fig. 14a), the parameters can be derived from the slope and intercept, which are summarized in Table 4. In the case of the metanil yellow dye adsorption onto the TM-CuNiZn–BDC MOF, both KT and β rise with an increase in temperature, indicating an endothermic process where adsorption becomes more favorable and stronger at higher temperatures.

Fig. 14. Comparative adsorption of various dyes onto CuNiZn–BDC MOF.

Fig. 14

3.5.4. Dubinin–Radushkevich (D–R) isotherm model

The D–R model is a dominant tool for characterizing adsorption onto dual surfaces, both homogeneous and heterogeneous, and is particularly useful for evaluating porosity-related adsorption and distinguishing between physisorption and chemisorption mechanisms. Mathematically, it can be presented as follows:

ln qe = ln qDR − γε2, 17
ε = RT ln(1 + 1/Ce). 18

The plot of ln qevs. ε (Fig. 11b) yields the values of γ and qDR. Eqn (19) is employed for the determination of the mean free energy change E utilizing the value of γ as follows:

3.5.4. 19
Fig. 11. Isotherm models applied to the adsorption of the metanil yellow dye on trimetallic CuNiZn–BDC MOF: (a) Temkin isotherm model and (b) Dubinin–Radushkevich D–R isotherm model.

Fig. 11

This energy value serves as an indicator of the mechanism of adsorption. E values below 8 kJ mol−1 indicate physisorption, while 8–16 kJ mol−1 signify chemisorption.48 Here, an increase in qDR with temperature and E values within 8–16 kJ mol−1 show that MY dye adsorption on CuNiZn–BDC MOF is mainly chemisorptive via ion exchange. Based on the equilibrium data and R2 value analysis, it was found that the Langmuir isotherm model best explained the adsorptive elimination of metanil yellow dye onto trimetallic CuNiZn–BDC MOF, as it exhibited a high regression coefficient (R2 = 0.992), which indicates monolayer adsorption of dye onto identical and energetically uniform binding active sites. In contrast, the Freundlich isotherm model (R2 = 0.923) and Temkin isotherm model (R2 = 0.973) showed inferior fits, suggesting that factors like surface heterogeneity, multilayer adsorption, and adsorbate–adsorbate interactions are not dominant in this adsorption system.49 These findings indicate that metanil yellow dye molecules occupy specific, homogeneous surface-active sites on the CuNiZn–BDC MOF, affirming the suitability of a monolayer adsorption mechanism under the investigated conditions (Fig. 12).

Fig. 12. van't Hoff plot of the adsorption of metanil yellow onto the TM-CuNiZn–BDC MOF.

Fig. 12

3.6. Statistical assessment of adsorption isotherm models

The Langmuir model gave the best fit for the experimental results at all temperatures investigated (293–333 K), with a correlation coefficient of 0.9942–0.9990 and a minimum value of RMSE and RSS as given in Table 4.50 The Freundlich model performed well, while the Temkin and Dubinin–Radushkevich (D–R) models had relatively high fitting errors.51 The results suggest that the Langmuir equation is the most suitable model to represent the adsorption equilibrium data.52

3.7. Thermodynamic study

The adsorption of metanil yellow dye on trimetallic CuNiZn–BDC MOF was studied at three temperatures, 293, 323 and 323 K. The results revealed that the extent of adsorption increases with an increase in the temperature of the medium. To investigate the feasibility of adsorption, thermodynamic parameters such as free energy (ΔG°), enthalpy (ΔH°) and entropy (ΔS°) changes were evaluated by the following equation:

3.7. 20

where R is the universal gas constant (8.314 J K−1 mol−1), T is the absolute temperature (K) and kc is the equilibrium constant. The equilibrium constant, kc, for the adsorption process was determined using the method reported by Debnath et al.53 ΔS° and ΔH° represent the standard entropy and enthalpy changes, respectively. These thermodynamic parameters can be determined from the intercept and slope of the ln kdversus 1/T plot, and these values are subsequently used to calculate the Gibbs free energy change ΔG° at each studied temperature54 as follows:

ΔG° = ΔH° − TΔS°. 21

The thermodynamic investigation of metanil yellow adsorption onto the CuNiZn–BDC MOF (Fig. 15) revealed a positive enthalpy change, indicating the endothermic behavior of the process and revealing that adsorption efficiency improves at high temperatures. Concurrently, the positive change in entropy ΔS° suggests increased randomness at the solid–liquid boundary, probably caused by the replacement of solvent molecules and greater molecular disorder upon binding.50 A negative value for Gibbs free energy (ΔG°) at all temperatures indicates the spontaneity of the current adsorption process, with decreasing ΔG° magnitudes at higher temperatures reflecting enhanced spontaneity and stronger adsorbate–adsorbent interactions as thermal energy helps overcome activation barriers.55 The Arrhenius activation energy (Ea = 42.351 kJ mol−1) was obtained from the temperature-dependent pseudo-second-order rate constants (k2) and indicated that the adsorption process has a moderate energy barrier. The relatively high Ea value combined with the increasing k2 values at higher temperatures and the endothermic nature of the adsorption process indicates that the adsorption process is primarily controlled by chemisorption (strong adsorption interactions between the adsorbate and the active sites of the CuNiZn–BDC MOF).

Fig. 15. Metanil yellow dye removal efficiency by the regenerated TM-CuNiZn–BDC MOF adsorbent.

Fig. 15

Overall, the values of ΔG° suggest that the process is predominantly physical in nature and is spontaneous, but adsorption mechanisms cannot be determined from only the ΔG° values (Table 5). The PSO kinetic model, D–R adsorption energy (8–16 kJ mol−1), and activation energy (Ea = 42.351 kJ mol−1) indicate the contribution of chemical interactions. Hence, it is likely that the adsorption mechanism is a combination of physisorption and chemisorption; the former contributes towards the spontaneity of the process and the latter to the strength and rate of the adsorption process.

Table 5. Parameters from the thermodynamic investigation of the adsorption of metanil yellow on the TM-CuNiZn–BDC MOF.

Parameter 293 K 313 K 333 K
ΔG° (kJ mol−1) −3.188 −4.397 −5.605
ΔH°(kJ mol−1) 14.511
ΔS° (J mol−1 K−1) 60.41
E a (kJ mol−1) 42.351

3.8. Comparative evaluation of the adsorption capacities for metanil yellow removal by different adsorbents

Table 6 presents the adsorption capacities of our TM-CuNiZn–BDC MOF alongside those reported in previous studies. The adsorptive efficiency of our adsorbent is substantially higher than most of the previously reported values, clearly demonstrating its strong potential for commercial-scale applications.

Table 6. Comparative evaluation of the MY dye adsorption capacities of the TM-CuNiZn–BDC MOF and reported adsorbents.

Adsorbent Maximum adsorption capacity, Qm Reference
Graphene oxide/chitosan biopolymer (3D-GCB) 157 mg g−1 56
Mg–Fe layered double hydroxide (LDH) 186 mg g−1 57
Modified shrimp shell (SS-PEI) 122 mg g−1 58
Cocoa pod shell magnetic nanoparticles 97 mg g−1 59
Manganese ferrite 271 mg g−1 60
Polyaniline-bentonite composite 444.4 mg g−1 61
Trimetallic CuNiZn–BDC MOF (present study) 689 mg g− 1 —

3.9. Comparison of the advantages of reported adsorbents with the present synthesized adsorbent

Table 7 presents a comparison of the advantages, experimental conditions and adsorption performance of the TM-CuNiZn–BDC MOF with those of previously reported adsorbents for the removal of metanil yellow. The synthesized trimetallic MOF showed a high Langmuir adsorption capacity of 689 mg g−1 and complete removal of the dye (more than 93%) within 60 min at pH 6 and 333 K. This adsorption capacity is greater than that of the biomass-based adsorbents, mesoporous silica and manganese ferrite materials reported previously. The good performance of the TM-CuNiZn–BDC MOF can be explained by the trimetallic composition, the relatively high BET surface area (654 m2 g−1) and the multiple potential interactions between the dye and the surface. However, the impact of variation in experimental conditions, as well as the observed decrease in removal efficiency during regeneration, should be taken into account when assessing its advantages for practice.

Table 7. Comparison of the advantages of reported adsorbents with the present synthesized adsorbent.

Adsorbent Maximum adsorption capacity Qmax (mg g−1) Reported conditions Key features or limitations Reference
Jatropha oil-cake biochar nanobiomaterial 24.3 pH 4; 90 min Low-cost biomass-derived material; dye recovery of up to 96.3% with acetone was reported 62
Water hyacinth leaves 170.8 pH 1.5–2.0 Renewable biosorbent; acidic conditions were required 63
Mesoporous silica (MCM-41) 172.4 90 min Ordered mesoporous structure; pseudo-second-order kinetic fit was reported 64
Chemically mediated manganese ferrite 271.89 100 min; pH 5 Magnetic ferrite material 65
Green-synthesized manganese ferrite 391.34 90 min; pH 4 Higher reported capacity than chemically mediated manganese ferrite in the same report 66
Pilot-scale super-activated carbon 537 pH 3; 303 K Very high reported capacity; pilot-scale production was demonstrated, but desorption/regeneration is needed 67
TM-CuNiZn–BDC MOF (present study) 689 pH 6; 333 K; 60 min Trimetallic MOF; BET surface area 654 m 2 g −1 ; removal efficiency above 93% under the reported optimum conditions Present study

3.10. Comparison of the adsorption efficiency of the TM-CuNiZn–BDC MOF with monometallic Cu–BDC, Ni–BDC and Zn–BDC MOFs

The adsorption efficiency of the monometallic and trimetallic BDC-based MOFs was in the order CuNiZn–BDC MOF > Cu–BDC MOF > Ni–BDC MOF > Zn–BDC MOF over the contact time range of 10–60 min (Fig. 13). The maximum adsorption capacities were about 184, 169, 161 and 153 mg g−1 at 60 min. The outstanding performance of the trimetallic MOF can be explained by the synergistic effect of Cu, Ni and Zn centers that can change the surface properties and also make the adsorption sites more available for the metanil yellow molecules. π–π interactions, electrostatic attraction and hydrogen bonding can play a role in dye uptake, which may occur between the aromatic BDC linkers. The structural and surface properties of CuNiZn–BDC MOF also demonstrate that the structure of CuNiZn–BDC MOF is more stable than that of Cu–BDC MOF, indicating possible synergistic effects, but additional analyses are needed to confirm these effects. Overall, the results suggest the feasibility of the trimetallic MOF design for better adsorption of metanil yellow.

Fig. 13. Comparison of the adsorption efficiency of the TM-CuNiZn–BDC MOF with monometallic Cu–BDC, Ni–BDC and Zn–BDC MOF.

Fig. 13

3.11. Comparative adsorption of various dyes onto CuNiZn–BDC MOF

Methylene blue (MB), metanil yellow (MY), Congo red (CR) and rhodamine blue (RhB) adsorption onto CuNiZn–BDC MOF showed a gradual increase with contact time from 10 to 60 min, suggesting that the available adsorption sites were occupied gradually (Fig. 14). MY showed the highest adsorption capacity of about 184 mg g−1 followed by MB (179 mg g−1), CR (171 mg g−1) and RB (163 mg g−1) at 60 min among the tested dyes. The difference could be due to the structure and size of the dye molecules, as well as the functional groups of the dye and the interactions between the MOF surface and the dye. The porous structure and the availability of adsorption sites in CuNiZn–BDC MOF are responsible for its adsorption performance, while electrostatic interactions, hydrogen bonding, and π–π interactions between the dye molecules and BDC aromatic rings could be responsible for the adsorption of the dye. Overall, CuNiZn–BDC MOF is a potential dye adsorbent material for dyes with different structural and chemical characteristics.

3.12. Regeneration and reusability of the TM-CuNiZn–BDC MOF

To assess the practicality of the TM-CuNiZn–BDC MOF for industrial-scale use and its capacity for repeated dye removal, a reusability test was carried out over seven adsorption–desorption cycles using metanil yellow. After each adsorption phase, the MOF was regenerated using a sequence of 0.1 M NaOH, acetone, and ethanol washes to desorb bound dye.68 As shown in Fig. 20, the MOF maintained nearly 75% dye removal efficiency for the first four cycles, indicating robust repeatability. However, subsequent cycles showed a gradual decline in performance, with the efficiency decreasing to 54% by the seventh cycle. The progressive decrease in performance may be associated with the incomplete regeneration of active sites, residual dye accumulation within the pores, and possible alterations of surface characteristics during repeated use. These results demonstrate that the synthesized TM-CuNiZn–BDC MOF exhibits moderate recyclability and retains a substantial portion of its adsorption capacity after multiple regenerations, making it a promising material for sustainable, repeated use in contaminated water treatment applications.

Fig. 20. SEM image of the metanil yellow-loaded CuNiZn–BDC MOF (MY@TM-CuNiZn–BDC MOF).

Fig. 20

Furthermore, the regeneration study showed that the CuNiZn–BDC MOF could be used in 7 cycles with 57.45% capacity retention from the initial capacity of 188 mg g−1. This step-wise degradation could be due to desorbed dye being incompletely removed, metal leaching, blocked adsorption sites, or changes occurring in the structure during dye regeneration. The EDX spectrum in Fig. 19 provides clues of metal leaching (Table 8).

Fig. 19. Elemental composition and EDX spectrum after the adsorption of metanil yellow onto TM-CuNiZn–BDC (MY@TM-CuNiZn–BDC).

Fig. 19

Table 8. Adsorption capacity and retention across seven regeneration cycles.

Cycle no. Removal (%) Adsorption capacity (mg g−1) Capacity retention (%)
1st 94 188.21 100
2nd 83 166.29 88.30
3rd 81 162.76 86.17
4th 74 148.34 78.72
5th 71 142.38 75.53
6th 62 124.97 65.96
7th 54 108.19 57.45

3.12.1. Mechanism of desorption

The desorption of metanil yellow dye from the CuNiZn–BDC MOF adsorbents is driven by several synergistic mechanisms that promote efficient regeneration, including solvent-induced disruption, ion-exchange displacement, pore restoration, and electrostatic weakening. In the solvent-induced disruption mechanism, organic solvents like ethanol and acetone penetrate the MOF pores and disrupt π–π interactions and break hydrogen bonds holding the dye molecules. In ion-exchange displacement, alkali cations (e.g., Na+ from NaOH solutions) compete with and replace the adsorbed dye via electrostatic interactions.69 Pore restoration occurs through solvent flushing that removes residual dye and reopens blocked channels, and electrostatic weakening occurs when alkaline wash treatments disrupt dye–CuNiZn–BDC MOF attraction by altering surface charge, collectively enabling complete dye removal and reuse of the MOF for multiple cycles.

3.13. Real wastewater treatment

The practical applicability of the synthesized CuNiZn–BDC MOF was then demonstrated by real textile wastewater with a dye content of about 130 mg L−1 and a pH of 5.8. The wastewater-treatment experiments were repeated three times for more reliable and reproducible results. The adsorption efficiency was also found to rise with increasing contact time, with the maximum adsorption efficiency being about 67% after 60 min, whereas about 94% removal in synthetic wastewater was achieved under similar contact time and experimental conditions, as shown in Fig. 16. The lower removal efficiency in the real wastewater matrix can be justified by the presence of co-existing pollutants, such as dissolved organic matter and ions that compete with the dye molecules for adsorption sites. Despite this, the high removal efficiency obtained in real wastewater shows that the synthesized adsorbent possesses good adsorption properties in complex aqueous solution, which indicates that it can be used in practice as a low-cost and efficient adsorbent for the treatment of textile wastewater.

Fig. 16. Adsorption performance in synthetic and real textile wastewater.

Fig. 16

3.14. Adsorption mechanism

The adsorption of metanil yellow dye onto CuNiZn–BDC MOF is governed by a synergistic combination of interactions facilitated by its porous structure and functional ligands (Fig. 17). Electrostatic attraction is a primary driver, as the anionic dye is drawn toward the MOF's positively charged surface under acidic conditions. Hydrogen bonding between carboxylate groups of the BDC linker (or coordinated water molecules) and functional moieties on the dye (C Created by potrace 1.16, written by Peter Selinger 2001-2019 O, –OH, and –NH2) further stabilizes binding; π–π stacking interactions occur between the aromatic rings of metanil yellow dye and the benzene ring of BDC, and dye–metal coordination also occurs.70 van der Waals forces contribute additional physisorptive stabilization within the pores, and the MOF's intrinsic porosity permits dye diffusion and entrapment within its channels. Cu2+ centers can offer good adsorptive sites and interact with the functional groups of dyes, while Ni2+ can help stabilize the framework of the material and disperse the active sites. The surface properties, and possibly the porosity and framework assembly, of the zeolite may be affected by Zn2+. In combination, these metal ions may provide various adsorption sites, which can facilitate the adsorption of metanil yellow.

Fig. 17. Proposed mechanism for the adsorption of the metanil yellow dye onto the TM-CuNiZn–BDC MOF.

Fig. 17

3.15. Post-adsorption characterization

3.15.1. FTIR analysis

The FTIR spectrum (Fig. 18) of the metanil yellow-loaded CuNiZn–BDC MOF shows several characteristic absorption bands, which indicate possible interactions between the dye and the MOF. The wider band around 3200 to 3500 cm−1 may be due to the stretching of the O–H bond, and the changes in the bandwidth could be due to hydrogen bonding. The bands between 1500 and 1650 cm−1 could be related to C Created by potrace 1.16, written by Peter Selinger 2001-2019 C vibrations in the aromatic part of the molecule, while bands in the range of 1350–1450 cm−1 could be related to vibrations of the carboxylate groups and/or the aromatic groups, which might overlap with azo group vibrations. The bands between 1000 and 1250 cm−1 could be attributed to the sulfonate (–SO3−) stretching vibration of metanil yellow, indicating interactions between the anionic groups of the dye and the MOF surface. In addition, the adsorption process may take place by π–π stacking between the aromatic rings of the dye and those of the BDC linkers, and electrostatic attraction between the anionic dye groups and the positive sites on the surface, depending on the pH of the solution. Other interactions such as ion exchange or specific chemical reactions can also be responsible for dye absorption, but these interactions should be supported by comparison with the neat MOF spectrum and complementary analyses.

Fig. 18. Post-adsorption FTIR spectrum of TM-CuNiZn–BDC.

Fig. 18

3.15.2. EDX analysis

The EDX spectrum (Fig. 19) and elemental mapping (Fig. S11) for the MY-loaded CuNiZn–BDC MOF confirm the presence of C, N, O, Cu, Ni, Zn, and also S, which is associated with the MY dye adsorbed to the MOF. The presence of S supports the successful attachment of MY dye to the MOF surface. The relative signal intensities of the framework metal ions (Cu, Ni and Zn) were slightly decreased after the adsorption, which can be explained by the occurrence of minor metal leaching during the aqueous adsorption process and may be attributed to partial interaction of the framework with the solution. However, the typical signals of Cu, Ni, and Zn were still found, which implies that the trimetallic structure was preserved to a large extent following adsorption. As a whole, the EDX results support MY uptake and suggest some surface compositional changes in the MOF.

3.15.3. Scanning electron microscopy

The SEM image (Fig. 20) of the CuNiZn–BDC MOF (after metanil yellow adsorption) shows a rough and heterogeneous surface, with irregularly shaped particles exhibiting significant agglomeration. The particle aggregates are seen to have different sizes and interparticle voids and irregularities on the surface. All the above-mentioned morphological features indicate that the surface of the MOF is not homogeneous and can promote interactions between the MOF and the dye molecules. After adsorption, it is possible that the surface is not completely covered and some of the available adsorption sites are not accessible because of dye molecule accumulation.

4. Conclusions

In summary, the TM-CuNiZn–BDC MOF was successfully fabricated using a solvothermal approach and demonstrated outstanding ability to adsorb and remove metanil yellow dye from aqueous solutions. Physicochemical characterization was comprehensively performed, which confirmed that the MOF has a rough surface morphology with spherical particles, essential functional groups, a microporous structure (632 m2 g−1), high specific surface area, and thermal stability up to 600 °C. Under optimal conditions (0.01 g adsorbent, pH 6, 200 mg per L dye, 60 minutes), the adsorption of MY on the TM-CuNiZn–BDC MOF was described using the pseudo-second-order kinetic and Langmuir isotherm models. The chemisorption was predominant, and the maximum capacity of the monolayer adsorption was 689 mg g−1 at 333 K. It was a spontaneous, endothermic process, and the MOF could operate at 64% capacity following seven cycles of reuse, which indicated that the MOF was sufficiently effective in terms of industrial application in dye removal.

Author contributions

AU, SA, FMA, MI and MZ are all equal contributors to the experiment, conceptualization, literature survey and MS writing. All authors have approved the final draft paper for submission.

Conflicts of interest

The authors declared that they have no known competing financial interests or personal relationships that could affect the work presented in this paper.

Supplementary Material

RA-OLF-D6RA09329A-s001

Acknowledgments

The authors express their gratitude to Princess Nourah bint Abdulrahman University Researchers Supporting Project number (PNURSP2026R42), Princess Nourah bint Abdulrahman University, Riyadh, Saudi Arabia.

Data availability

All data are presented in this manuscript. There are no associated data in any repository.

Supplementary information (SI) is available. See DOI: https://doi.org/10.1039/d6ra09329a.

References

  1. Islam T. Repon M. R. Islam T. Sarwar Z. Rahman M. M. Impact of textile dyes on health and ecosystem: a review of structure, causes, and potential solutions. Environ. Sci. Pollut. Res. 2023;30(4):9207–9242. doi: 10.1007/s11356-022-24398-3. [DOI] [PubMed] [Google Scholar]
  2. De Oliveira D. P., Zanoni M., Chequer F., Oliveira G., Cardoso J. and Ferraz E., Textile dyes: dyeing process and environmental impact, Eco-Friendly Textile Dyeing and Finishing, 2013, p. 151 [Google Scholar]
  3. Jain R. Sharma N. Radhapyari K. Removal of hazardous azo dye metanil yellow from industrial wastewater using electrochemical technique. Eur. Water. 2009;27(28):43–52. [Google Scholar]
  4. Sadiq M. Ullah I. Iqbal Z. Wahid A. Umar A. Iqbal Z. et al., Preparation and characterization of catalysts and its application in microwave-assisted degradation of acid orange-8. Desalin. Water Treat. 2021;231:407–414. doi: 10.5004/dwt.2021.27450. [DOI] [Google Scholar]
  5. Isiuku B. Anyanwu D. Nwosu C. Iroamaka S. Batch adsorptive removal of metanil yellow from simulated dye wastewater using nitric acid modified-H3PO4-activated carbon (NAMPAAC) from Gmelina arborea bark: equilibrium and isotherm studies. Desalin. Water Treat. 2017;70:380–386. doi: 10.5004/dwt.2017.20510. [DOI] [Google Scholar]
  6. Crini G. Lichtfouse E. Advantages and disadvantages of techniques used for wastewater treatment. Environ. Chem. Lett. 2019;17(1):145–155. doi: 10.1007/s10311-018-0785-9. [DOI] [Google Scholar]
  7. Rashid R. Shafiq I. Akhter P. Iqbal M. J. Hussain M. A state-of-the-art review on wastewater treatment techniques: the effectiveness of adsorption method. Environ. Sci. Pollut. Res. 2021;28(8):9050–9066. doi: 10.1007/s11356-021-12395-x. [DOI] [PubMed] [Google Scholar]
  8. Satyam S. Patra S. Innovations and challenges in adsorption-based wastewater remediation: A comprehensive review. Heliyon. 2024;10(9):e29573. doi: 10.1016/j.heliyon.2024.e29573. [DOI] [PMC free article] [PubMed] [Google Scholar]
  9. Adeyemo A. A. Adeoye I. O. Bello O. S. Adsorption of dyes using different types of clay: a review. Appl. Water Sci. 2017;7(2):543–568. doi: 10.1007/s13201-015-0322-y. [DOI] [Google Scholar]
  10. Iyer E. S. S., Smart and intelligent bionanomaterials as adsorbents for management of heavy metal–polluted wastewater, Nanobiotechnology for Bioremediation, Elsevier, 2023, pp. 181–213 [Google Scholar]
  11. Zeeshan M. Javed T. Kumari C. Thumma A. Wasim M. Taj M. B. Sharma I. Haider M. N. Batool M. Investigating the interactions between dyes and porous/composite materials: A comprehensive study. Sustainable Chem. Environ. 2025;9:100217. doi: 10.1016/j.scenv.2025.100217. [DOI] [Google Scholar]
  12. Al-Jubouri S. M. Al-Batty S. Al-Hamd R. K. S. Sims R. Hakami M. W. SK M. H. Sustainable environment through using porous materials: A review on wastewater treatment. Asia-Pac. J. Chem. Eng. 2023;18(4):e2941. doi: 10.1002/apj.2941. [DOI] [Google Scholar]
  13. Gul Zaman H. Baloo L. Pendyala R. Singa P. K. Ilyas S. U. Kutty S. R. M. Produced water treatment with conventional adsorbents and MOF as an alternative: A review. Materials. 2021;14(24):7607. doi: 10.3390/ma14247607. [DOI] [PMC free article] [PubMed] [Google Scholar]
  14. Adeyemo A. A. Adeoye I. O. Bello O. S. Metal organic frameworks as adsorbents for dye adsorption: overview, prospects and future challenges. Toxicol. Environ. Chem. 2012;94(10):1846–1863. doi: 10.1080/02772248.2012.744023. [DOI] [Google Scholar]
  15. Luo X. Abazari R. Tahir M. Fan W. K. Kumar A. Kalhorizadeh T. et al., Trimetallic metal–organic frameworks and derived materials for environmental remediation and electrochemical energy storage and conversion. Coord. Chem. Rev. 2022;461:214505. doi: 10.1016/j.ccr.2022.214505. [DOI] [Google Scholar]
  16. Al-Omari M. H. Abu-Rayyan A. Ragab A. H. Taher M. A. El-Sayed E.-S. M. Elfiky A. et al., Optimized Congo red dye adsorption using ZnCuCr-based MOF for sustainable wastewater treatment. Langmuir. 2025;41(9):5947–5961. doi: 10.1021/acs.langmuir.4c04661. [DOI] [PubMed] [Google Scholar]
  17. Sahiner N. Demirci S. Yildiz M. Preparation and characterization of bi-metallic and tri-metallic metal organic frameworks based on trimesic acid and Co (II), Ni (II), and Cu (II) ions. J. Electron. Mater. 2017;46(2):790–801. doi: 10.1007/s11664-016-4969-4. [DOI] [Google Scholar]
  18. Umar A. Alam S. Zaman H. Zahoor M. Ullah R. Ali E. A. et al., Facile Synthesis and Characterization of Trimetallic CuCrFe-BTC MOF for the Adsorptive Removal of Diamond Green G: Kinetic, Isotherm, and Thermodynamic Study. Appl. Organomet. Chem. 2025;39(6):e70189. doi: 10.1002/aoc.70189. [DOI] [Google Scholar]
  19. Ghaedi M. Hajjati S. Mahmudi Z. Tyagi I. Agarwal S. Maity A. et al., Modeling of competitive ultrasonic assisted removal of the dyes–Methylene blue and Safranin-O using Fe3O4 nanoparticles. Chem. Eng. J. 2015;268:28–37. doi: 10.1016/j.cej.2014.12.090. [DOI] [Google Scholar]
  20. Kim H.-G. Choi K. Lee K. Lee S. Jung K.-W. Choi J.-W. Controlling the structural robustness of zirconium-based metal organic frameworks for efficient adsorption on tetracycline antibiotics. Water. 2021;13(13):1869. doi: 10.3390/w13131869. [DOI] [Google Scholar]
  21. Bakhtiari N. Azizian S. Nanoporous carbon derived from MOF-5: a superadsorbent for copper ions. ACS Omega. 2018;3(12):16954. doi: 10.1021/acsomega.8b02278. [DOI] [PMC free article] [PubMed] [Google Scholar]
  22. Deng Z. Cao J. Zhao L. Zhang Z. Yuan J. Trimetallic FeCoNi metal–organic framework with enhanced peroxidase-like activity for the construction of a colorimetric sensor for rapid detection of thiophenol in water samples. Molecules. 2024;29(16):3739. doi: 10.3390/molecules29163739. [DOI] [PMC free article] [PubMed] [Google Scholar]
  23. Abid H. R. Rada Z. H. Shang J. Wang S. Synthesis, characterization, and CO2 adsorption of three metal-organic frameworks (MOFs): MIL-53, MIL-96, and amino-MIL-53. Polyhedron. 2016;120:103–111. doi: 10.1016/j.poly.2016.06.034. [DOI] [Google Scholar]
  24. Hamdalla T. A. Alfadhli S. Khasim S. Darwish A. ElZaidia E. Al-Ghamdi S. et al., Synthesis of novel Cu/Fe based benzene Dicarboxylate (BDC) metal organic frameworks and investigations into their optical and electrochemical properties. Heliyon. 2024;10(3):e25065. doi: 10.1016/j.heliyon.2024.e25065. [DOI] [PMC free article] [PubMed] [Google Scholar]
  25. Latrach Z. Moumen E. Kounbach S. El Hankari S. Mixed-ligand strategy for the creation of hierarchical porous ZIF-8 for enhanced adsorption of copper ions. ACS Omega. 2022;7(18):15862. doi: 10.1021/acsomega.2c00980. [DOI] [PMC free article] [PubMed] [Google Scholar]
  26. Peng M. M. Jeon U. J. Ganesh M. Aziz A. Vinodh R. Palanichamy M. et al., Oxidation of Ethylbenzene Using Nickel Oxide Supported Metal Organic Framework Catalyst. Bull. Korean Chem. Soc. 2014;35(11):3213. doi: 10.5012/bkcs.2014.35.11.3213. [DOI] [Google Scholar]
  27. Challa M. Chinnam S. Rajanna A. M. Nandagudi A. Yallur B. C. Adimule V. Adsorption efficacy of functionalized Cu-BDC MOFs tethered 2-mercaptobenzimidazole analogue: A comparative study. Heliyon. 2023;9(2):e13223. doi: 10.1016/j.heliyon.2023.e13223. [DOI] [PMC free article] [PubMed] [Google Scholar]
  28. Al-Harbi S. A. Almulaiky Y. Q. Copper-based metal-organic frameworks (BDC-Cu MOFs) as supporters for α-amylase: Stability, reusability, and antioxidant potential. Heliyon. 2024;10(6):e28396. doi: 10.1016/j.heliyon.2024.e28396. [DOI] [PMC free article] [PubMed] [Google Scholar]
  29. Yarahmadi H. Salamah S. K. Kheimi M. Synthesis of an efficient MOF catalyst for the degradation of OPDs using TPA derived from PET waste bottles. Sci. Rep. 2023;13(1):19136. doi: 10.1038/s41598-023-46635-6. [DOI] [PMC free article] [PubMed] [Google Scholar]
  30. Omkaramurthy B. Krishnamurthy G. Prasad N. Two new Zn (II) bdc Metal-Organic Frameworks based on benzene 1, 4-dicarboxylic acid: Synthesis, Crystal structures, Luminescent properties and Electrochemical studies. Mater. Today: Proc. 2020;22:2179–2190. [Google Scholar]
  31. Nurmi J. T. Tratnyek P. G. Sarathy V. Baer D. R. Amonette J. E. Pecher K. et al., Characterization and properties of metallic iron nanoparticles: spectroscopy, electrochemistry, and kinetics. Environ. Sci. Technol. 2005;39(5):1221–1230. doi: 10.1021/es049190u. [DOI] [PubMed] [Google Scholar]
  32. Li H. Eddaoudi M. O'Keeffe M. Yaghi O. M. Design and synthesis of an exceptionally stable and highly porous metal-organic framework. Nature. 1999;402(6759):276–279. doi: 10.1038/46248. [DOI] [Google Scholar]
  33. Abd El Salam H. Bio-sustainable alternatives synthesis of nanoporous activated carbon@ Al-MOF for the adsorption of hazardous organic dyes from wastewater. Water, Air, Soil Pollut. 2023;234(9):567. doi: 10.1007/s11270-023-06572-6. [DOI] [Google Scholar]
  34. Yang L. Xue N. Zhang W. He H. Influences of pH and NaCl on metanil yellow decolouration by adsorption and photocatalytic decolouration. Asian J. Chem. 2015:210–212. doi: 10.14233/ajchem.2015.16868. [DOI] [Google Scholar]
  35. Yadav B. S. Dasgupta S. Effect of time, pH, and temperature on kinetics for adsorption of methyl orange dye into the modified nitrate intercalated MgAl LDH adsorbent. Inorg. Chem. Commun. 2022;137:109203. doi: 10.1016/j.inoche.2022.109203. [DOI] [Google Scholar]
  36. Nadafi K. Vosoughi M. Asadi A. Borna M. O. Shirmardi M. Reactive Red 120 dye removal from aqueous solution by adsorption on nano-alumina. J. Water Chem. Technol. 2014;36(3):125–133. doi: 10.3103/S1063455X14030059. [DOI] [Google Scholar]
  37. Nandi B. K. Patel S. Effects of operational parameters on the removal of brilliant green dye from aqueous solutions by electrocoagulation. Arabian J. Chem. 2017;10:S2961–S2968. doi: 10.1016/j.arabjc.2013.11.032. [DOI] [Google Scholar]
  38. Umar A. Khan M. S. Alam S. Zekker I. Burlakovs J. dC Rubin S. S. et al., Synthesis and characterization of Pd-Ni bimetallic nanoparticles as efficient adsorbent for the removal of acid orange 8 present in wastewater. Water. 2021;13(8):1095. doi: 10.3390/w13081095. [DOI] [Google Scholar]
  39. Alam S. Khan M. S. Umar A. Khattak R. Rahman N. U. Zekker I. et al., Preparation of Pd–Ni nanoparticles supported on activated carbon for efficient removal of basic blue 3 from water. Water. 2021;13(9):1211. doi: 10.3390/w13091211. [DOI] [Google Scholar]
  40. Umar A. Alam S. ur Rehman N. Zahoor M. Ullah R. Ali E. A. et al., Synthesis of trimetallic; CuNiZn-BTC MOF for the removal of patent blue VF dye from aqueous solutions. Inorg. Chem. Commun. 2025;180:114942. doi: 10.1016/j.inoche.2025.114942. [DOI] [Google Scholar]
  41. Eltaweil A. S. Abd El-Monaem E. M. Omer A. M. Khalifa R. E. Abd El-Latif M. M. El-Subruiti G. M. Efficient removal of toxic methylene blue (MB) dye from aqueous solution using a metal-organic framework (MOF) MIL-101 (Fe): Isotherms, kinetics, and thermodynamic studies. Desalin. Water Treat. 2020;189:395–407. doi: 10.5004/dwt.2020.25599. [DOI] [Google Scholar]
  42. Wu F.-C. Tseng R.-L. Juang R.-S. Characteristics of Elovich equation used for the analysis of adsorption kinetics in dye-chitosan systems. Chem. Eng. J. 2009;150(2–3):366–373. doi: 10.1016/j.cej.2009.01.014. [DOI] [Google Scholar]
  43. Pandian A. M. K. Karthikeyan C. Rajasimman M. Isotherm and kinetic studies on adsorption of malachite green using chemically synthesized silver nanoparticles. Nanotechnol. Environ. Eng. 2017;2(1):2. doi: 10.1007/s41204-016-0013-4. [DOI] [Google Scholar]
  44. Ali D. A. Saad F. A. Elsawy H. A. Kinetics and isotherm studies for adsorption of gentian violet dye from aqueous solutions using synthesized hydroxyapatite. J. Environ. Public Health. 2023;2023(1):7418770. doi: 10.1155/2023/7418770. [DOI] [PMC free article] [PubMed] [Google Scholar]
  45. Gimbert F. Morin-Crini N. Renault F. Badot P.-M. Crini G. Adsorption isotherm models for dye removal by cationized starch-based material in a single component system: error analysis. J. Hazard. Mater. 2008;157(1):34–46. doi: 10.1016/j.jhazmat.2007.12.072. [DOI] [PubMed] [Google Scholar]
  46. Shiri M. Hosseinzadeh M. Shiri S. Javanshir S. Adsorbent based on MOF-5/cellulose aerogel composite for adsorption of organic dyes from wastewater. Sci. Rep. 2024;14(1):15623. doi: 10.1038/s41598-024-65774-y. [DOI] [PMC free article] [PubMed] [Google Scholar]
  47. Ojediran J. O. Dada A. O. Aniyi S. O. David R. O. Adewumi A. D. Mechanism and isotherm modeling of effective adsorption of malachite green as endocrine disruptive dye using Acid Functionalized Maize Cob (AFMC) Sci. Rep. 2021;11(1):21498. doi: 10.1038/s41598-021-00993-1. [DOI] [PMC free article] [PubMed] [Google Scholar]
  48. Sevim F. Laçin Ö. Demir F. Erkiliç Ö. F. Adsorption capacity, isotherm, kinetics, and thermodynamics examinations on the removal of a textile azo dye by local natural adsorbent. Glob. Chall. 2025;9(5):2500024. doi: 10.1002/gch2.202500024. [DOI] [PMC free article] [PubMed] [Google Scholar]
  49. Aljeboree A. M. Alshirifi A. N. Alkaim A. F. Kinetics and equilibrium study for the adsorption of textile dyes on coconut shell activated carbon. Arabian J. Chem. 2017;10:S3381–S3393. doi: 10.1016/j.arabjc.2014.01.020. [DOI] [Google Scholar]
  50. Nasir M. Bharti M. Kashif M. Rahman N. Malik A. Siddiqi N. J. et al., Mechanistic Insights Into Nickel (II) Adsorption–Diffusion on Sulfamoylbenzamide-Modified Hydrous Zirconium Oxide for Wastewater Treatment. ChemistrySelect. 2026;11(9):e07348. doi: 10.1002/slct.202507348. [DOI] [Google Scholar]
  51. Nasir M. Sana Afroz A. Kashif M. Malik A. Siddiqi N. J. et al., Simultaneous adsorption of oxytetracycline and arsenic onto hydrous zirconium-modified chitosan/β-cyclodextrin composite: mechanistic insights via statistical physics modeling, fractal-like kinetics, thermodynamic evaluation, and site energy distribution analysis. New J. Chem. 2026;50(8):3643–3665. doi: 10.1039/D5NJ03795F. [DOI] [Google Scholar]
  52. Afroz A. Nasir M. Kashif M. Samdani M. S. Green approach for the synthesis of a acrylonitrile hyperbranched polymer/chitosan composite for the removal of diclofenac from water: determination of optimal conditions using statistical experiment design. New J. Chem. 2024;48(46):19621–19637. doi: 10.1039/D4NJ04068F. [DOI] [Google Scholar]
  53. Debnath S. Maity A. Pillay K. Magnetic chitosan–GO nanocomposite: Synthesis, characterization and batch adsorber design for Cr (VI) removal. J. Environ. Chem. Eng. 2014;2(2):963–973. doi: 10.1016/j.jece.2014.03.012. [DOI] [Google Scholar]
  54. Rahman N. Nasir M. Development of Zr (IV)—Doped polypyrrole/zirconium (IV) iodate composite for efficient removal of fluoride from water environment. J. Water Proc. Eng. 2017;19:172–184. doi: 10.1016/j.jwpe.2017.07.016. [DOI] [Google Scholar]
  55. Gunasekar V. Ponnusami V. Kinetics, equilibrium, and thermodynamic studies on adsorption of methylene blue by carbonized plant leaf powder. J. Chem. 2013;2013(1):415280. doi: 10.1155/2013/415280. [DOI] [Google Scholar]
  56. Sahmoune M. N. Evaluation of thermodynamic parameters for adsorption of heavy metals by green adsorbents. Environ. Chem. Lett. 2019;17(2):697–704. doi: 10.1007/s10311-018-00819-z. [DOI] [Google Scholar]
  57. Lai K. C. Tee W. T. Li Loh N. Y. Hiew B. Y. Z. Gan S. Lee L. Y. Continuous adsorption of Metanil Yellow and Remazol Black B dyes onto ifxed-bed of 3D graphene oxide/chitosan biopolymer. S. Afr. J. Chem. Eng. 2024;48(1):276–284. [Google Scholar]
  58. Nejati K. Rezvani Z. Mansurfar M. Mirzaee A. Mahkam M. Adsorption of metanil yellow azoic dye from aqueous solution onto Mg-Fe-NO3 layered double hydroxide. Z. Anorg. Allg. Chem. 2011;637(11):1573–1579. doi: 10.1002/zaac.201100132. [DOI] [Google Scholar]
  59. Zein R. Chaidir Z. Zilfa Z. Fauzia S. Ramadhani P. Isotherm and kinetic studies on the adsorption behavior of metanil yellow dyes onto modified shrimp shell-polyethylenimine (SS-PEI) J. Kim. Valensi. 2022:10–22. doi: 10.15408/jkv.v8i1.22566. [DOI] [Google Scholar]
  60. Omer M. Khan B. Khan I. Alamzeb M. Zada F. M. Ullah I. et al., Equilibrium, kinetic and thermodynamic studies for the adsorption of metanil yellow using carbonized pistachio shell-magnetic nanoparticles. Water. 2022;14(24):4139. doi: 10.3390/w14244139. [DOI] [Google Scholar]
  61. Sivashankar R. Sivasubramanian V. Kishore K. A. Sathya A. B. Thirunavukkarasu A. Nithya R. et al., Metanil Yellow dye adsorption using green and chemical mediated synthesized manganese ferrite: An insight into equilibrium, kinetics and thermodynamics. Chemosphere. 2022;307:136218. doi: 10.1016/j.chemosphere.2022.136218. [DOI] [PubMed] [Google Scholar]
  62. Vyas D. Rathod M. Khambhaty Y. Basha S. Sustainable removal of metanil yellow from aqueous systems via adsorption on Jatropha biodiesel cake nanobiomaterial. Indian J. Chem. Technol. 2026;33(2):217–227. [Google Scholar]
  63. Aranda-García E. Guerrero-Coronilla I. Cristiani-Urbina E. Water hyacinth leaves are an efficient, green, and cost-effective biosorbent for the removal of metanil yellow from aqueous solution: kinetics, isotherm, and thermodynamic studies. Molecules. 2024;29(14):3409. doi: 10.3390/molecules29143409. [DOI] [PMC free article] [PubMed] [Google Scholar]
  64. Indriani I. Taba Samriani P. Synthesis and characterization of mesoporous silica as adsorbent for metanil yellow dye. AIP Conf. Proc. 2024;2774:030017. doi: 10.1063/5.0164494. [DOI] [Google Scholar]
  65. Sawant S. Y. Pawar R. R. Senthilkumar S. Somani R. S. Cho M. H. Bajaj H. C. Pilot-scale produced super activated carbon with a nanoporous texture as an excellent adsorbent for the efficient removal of metanil yellow. Powder Technol. 2018;333:243–251. doi: 10.1016/j.powtec.2018.04.024. [DOI] [Google Scholar]
  66. Meng F. Wang L. Pei M. Guo W. Liu G. Adsorption of metanil yellow from aqueous solution using polyaniline-bentonite composite. Colloid Polym. Sci. 2017;295(7):1165–1175. doi: 10.1007/s00396-017-4098-5. [DOI] [Google Scholar]
  67. Paiman S. H. Rahman M. A. Uchikoshi T. Abdullah N. Othman M. H. D. Jaafar J. et al., Functionalization effect of Fe-type MOF for methylene blue adsorption. J. Saudi Chem. Soc. 2020;24(11):896–905. doi: 10.1016/j.jscs.2020.09.006. [DOI] [Google Scholar]
  68. Sağlam S. Türk F. N. Arslanoğlu H. Use and applications of metal-organic frameworks (MOF) in dye adsorption. J. Environ. Chem. Eng. 2023;11(5):110568. doi: 10.1016/j.jece.2023.110568. [DOI] [Google Scholar]
  69. Beydaghdari M. Hooriabad Saboor F. Babapoor A. Karve V. V. Asgari M. Recent advances in MOF-based adsorbents for dye removal from the aquatic environment. Energies. 2022;15(6):2023. doi: 10.3390/en15062023. [DOI] [Google Scholar]
  70. Kaur H. Devi N. Siwal S. S. Alsanie W. F. Thakur M. K. Thakur V. K. Metal–organic framework-based materials for wastewater treatment: superior adsorbent materials for the removal of hazardous pollutants. ACS Omega. 2023;8(10):9004. doi: 10.1021/acsomega.2c07719. [DOI] [PMC free article] [PubMed] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

RA-OLF-D6RA09329A-s001

Data Availability Statement

All data are presented in this manuscript. There are no associated data in any repository.

Supplementary information (SI) is available. See DOI: https://doi.org/10.1039/d6ra09329a.


Articles from RSC Advances are provided here courtesy of Royal Society of Chemistry