Abstract
Thermoelectric materials generate electric energy from waste heat, with conversion efficiency governed by the dimensionless figure of merit, ZT. Single-crystal tin selenide (SnSe) was discovered to exhibit a high ZT of roughly 2.2–2.6 at 913 K, but more practical and deployable polycrystal versions of the same compound suffer from much poorer overall ZT, thereby thwarting prospects for cost-effective lead-free thermoelectrics. The poor polycrystal bulk performance is attributed to traces of tin oxides covering the surface of SnSe powders, which increases thermal conductivity, reduces electrical conductivity and thereby reduces ZT. Here, we report that hole-doped SnSe polycrystalline samples with reagents carefully purified and tin oxides removed exhibit an ZT of roughly 3.1 at 783 K. Its lattice thermal conductivity is ultralow at roughly 0.07 W m–1 K–1 at 783 K, lower than the single crystals. The path to ultrahigh thermoelectric performance in polycrystalline samples is the proper removal of the deleterious thermally conductive oxides from the surface of SnSe grains. These results could open an era of high-performance practical thermoelectrics from this high-performance material.
Subject terms: Solid-state chemistry, Thermoelectrics
SnSe has a very high thermoelectric figure of merit ZT, but uncommonly polycrystalline samples have higher lattice thermal conductivity than single crystals. Here, by controlling Sn reagent purity and removing SnOx impurities, a lower thermal conductivity is achieved, enabling ZT of 3.1 at 783 K.
Main
More than 65% of the globally produced energy is lost as waste heat1. Thermoelectric power generators are semiconductor-based electronic devices that can turn such waste heat into electricity through the Seebeck effect2. This conversion process is free of motion or moving parts, thus can be an eco-friendly solution to recovering and using enormous amounts of waste heat to create electricity. The efficiency of thermoelectric semiconductors is assessed by the dimensionless figure of merit ZT = S2σT/κtot (refs. 2–4), where S is the Seebeck coefficient, σ is the electrical conductivity, T is the absolute temperature and κtot is the total thermal conductivity from the electrical (κele) and lattice vibration contribution (κlat)3.
ZT values have been substantially improved by developing various strategies for increasing power factor (the product S2σ) or suppressing κlat in the past decade. They have been individually or multiply applied to representative thermoelectric systems such as lead chalcogenides5, skutterudites6 and half-Heusler compounds7. For example, an unusually high ZT roughly 2.2–2.5 around 920 K was achieved in PbTe–SrTe systems by applying multiple strategies of band engineering, endotaxial nanostructuring, hierarchical architecturing and non-equilibrium processing8. However, among the state-of-the-art thermoelectric systems, the most surprising and promising is the discovery of tin selenide (SnSe) as a top thermoelectric material9–11. This material combines two very desirable attributes: (1) highly effective inherent ultralow thermal conductivity and (2) very favourable electronic band structure with multiple bands contributing to the charge transport, thereby contributing to the ultrahigh power factor9–11. The innate strongly anisotropic and anharmonic crystal chemistry gives rise to intrinsically ultralow κlat of roughly 0.20 W m–1 K–1. As a result, its p-type pristine crystals exhibit a ZT of 2.6 at 913 K along the b axis9, and the Br-doped n-type crystals show a ZT of 2.8 at 773 K along the a axis11.
However, these extraordinarily high thermoelectric properties have been only observable in single-crystal SnSe samples while the polycrystalline versions show much poorer figure of merit12–14. In fact, many research groups have observed much higher thermal conductivity κlat values in polycrystalline SnSe samples than those reported for the single-crystal samples, despite the expected presence of additional phonon scattering mechanism from the grain boundaries (GBs)15,16. Accordingly, ZT values of the polycrystalline SnSe materials have been much lower than those of the single crystals. This has led to controversy regarding the ultralow κlat of SnSe as an intrinsic property and whether the exceptional ZT values of the single-crystal SnSe can ever be achieved in polycrystalline SnSe samples15. Indeed, given the high cost, lengthy and labour-intensive production, poor mechanical brittleness and high cleavability of the single-crystal SnSe samples, it is the polycrystalline samples that have a realistic chance to achieve mass production and commercial applications. Consequently, it has been a huge challenge to realize comparable or even higher thermoelectric performance in polycrystalline SnSe samples. Indeed, matching single-crystal thermoelectric performance in polycrystalline SnSe would be a major development; not only because of both maximum and average ZT during operating temperature range, but also due to the relative abundance of Sn and Se (in comparison to Te) as well as the lead-free nature of the compound.
Recently, we have revealed that this apparently higher κlat reported for polycrystalline SnSe samples is attributed to the presence of surface tin oxides (SnOx) on SnSe powders12. SnO2 has approximately 140 times higher κlat than SnSe16. When the SnSe powders covered with SnOx thin films are compacted into dense pellets, high thermal conductivity SnOx present at GBs provides natural percolation pathway for heat transport. In this case, the thermal conductivity is greatly enhanced, contrary to the general expectation that polycrystalline samples should have lower thermal conductivity than that of their single-crystal counterpart due to expected extensive GB phonon scattering. In fact, high thermal conductivity SnOx phases can also easily grow on the surfaces of the single crystals, thereby often complicating the studies of the thermal transport properties. Further, the surface SnOx can strongly scatter charge carriers, consequentially affecting both thermal and charge transport properties adversely, and as a result severely curtailing the promise of a cost-effective, eco-friendly, widely deployable thermoelectric material such as SnSe. Indeed, polycrystalline SnSe with minimal GB and surface phase of SnOx would be a major advance in this context.
To initially mitigate this problem, we developed a postprocess of ball milling combined with chemical reduction for polycrystalline SnSe-based materials. This approach effectively removes SnOx phase from surfaces and subsequent interfaces to reveal the exceptionally low κlat of roughly 0.11 W m–1 K–1 and near-single-crystal ZT of roughly 2.5 at 773 K (ref. 12). However, despite this great progress these samples still show higher κlat of roughly 0.84–0.32 W m–1 K–1 than the single-crystal SnSe with 0.47–0.24 W m–1 K–1 in the nearly entire temperature range 300–673 K suggesting the presence of persistent and pervasive presence of SnOx in the samples. This continues to obscure the intrinsic thermal and charge-carrier transport properties of SnSe and, as a result, the true thermoelectric properties of SnSe have hitherto not yet been realized in polycrystalline samples of SnSe.
Herein, we report that the tin (Sn) metal starting reagent, despite its 99.999% purity, is the culprit behind the formation of surface SnOx in polycrystalline SnSe-based materials. To remedy this further, we have developed a facile and more efficient two-step process to remove the deleterious oxygen and minimize the presence of SnOx. Collectively, this further reduces the thermal conductivity and increases the power factor, thereby uncovering the extraordinarily high thermoelectric performance of polycrystalline SnSe, which reaches a ZT of roughly 3.1 at 783 K. A schematic illustration of this process is shown in Fig. 1.
Purification process for SnSe
As-received elemental tin (Sn) reagent must be purified before use. Note that we use 99.999% purity Sn chunks, showing a characteristic silvery lustre. This was chemically reduced by a 4% H2/Ar flow for 6 h at 473 K, near the melting point of Sn, showing no visible change in surface colour and lustre afterwards. The metal was subsequently heated at 1,223 K in an evacuated ampule. This caused ash-like black residues to form at the top and entire surface of the resulting Sn ingot and it was unambiguously identified as SnOx by far-infrared spectroscopy17 and atom probe tomography (APT) (Supplementary Figs. 1–3). After removing these residues, the melting-purification process was repeated until the ash-like black SnOx residues were no more visible. The purified Sn reagent was confirmed to be nearly oxygen-free according to the APT analysis (Supplementary Fig. 3). We found that the purification of elemental selenium (Se) reagent had a negligible influence on thermoelectric properties of SnSe. After the purification of Sn, the synthesized SnSe samples were pulverized and further purified under a 4% H2/96% Ar flow at 613 K for 6 h. For the sake of the discussion, samples prepared by this two-step purification process are referred to as ‘purified’, while those not prepared by this process are denoted as ‘untreated’.
Analysis of surface SnOx in untreated and purified SnSe
The facile formation of surface SnOx in polycrystalline SnSe samples is supported by our density functional theory (DFT) calculations (Supplementary Fig. 4 and Note). To probe the presence and distribution of surface SnOx in both the untreated and purified SnSe samples, we first performed time-of-flight–secondary ion mass spectrometry (TOF–SIMS). This is a highly surface-sensitive technique providing chemical mapping at spatial resolutions down to a submicrometre scale, thereby providing the broad-range distribution of surface SnOx at GBs. We mapped the SnOH+ species to reliably display the spatial distribution of tin-bound oxygen.
Figure 2a,b shows TOF–SIMS images of the untreated and purified spark plasma sintering (SPS) SnSe samples. Spread red spots correspond to the distribution of SnOH+, which are much fainter and less dense in the purified SnSe sample. The analysed data show that it has a factor of 7.4 lower SnOx concentration than the untreated sample. After identifying the GBs in the corresponding optical images (Supplementary Fig. 5a,b), the line-profile scan for the SnOx concentration was taken across them. It revealed that SnOx is more abundant in the GBs than in the interior regions of SnSe crystallites (Fig. 2c,d). This is not surprising in view of the compaction process of SnSe powders, which are surface-covered with SnOx.
We further investigated surface SnOx in GB regions in the untreated SnSe sample using a spherical aberration-corrected scanning transmission electron microscope (STEM). A representative high-angle annular dark-field (HAADF)–STEM image shows the presence of abundant nanoscale precipitates, indicated by the white arrows, around the GB marked by the orange dashed line and arrow (Fig. 3a). The corresponding elemental map reveals that they are rich in oxygen and devoid of selenium with the negligible fluctuation in the tin concentration throughout the specimen, thereby being identified as SnOx (Fig. 3b–e).
To spatially determine the distribution and composition of surface SnOx, we conducted APT analysis on the untreated SnSe sample. It quantitatively provides the three-dimensional distribution of constituent elements with equal sensitivity at a spatial resolution nearly down to the subatomic level, thereby serving as an effective tool to resolve secondary phases either in the matrix or trapped at GBs18–20. Figure 3f displays the three-dimensional reconstruction of the needle-shaped specimen from the untreated SnSe sample. The GB, marked by the orange arrow and dash line, is located by a much higher atomic counts due to the local magnification effect20. The high concentration O atoms are aggregated along the GB, coincident with our STEM observations. They also percolate into the grain forming SnOx layers as observed in the upper area in Fig. 3f.
To quantitatively resolve their content with the greater statistical accuracy, one-dimensional compositional profiles were recorded at the oxygen-rich region, namely both across the GB as enclosed by the blue cylinder (Fig. 3g) and across the oxygen-rich layer as marked by the green cylinder (Fig. 3h) in Fig. 3f. In these regions, the O concentration exceeds roughly 15 at% with a maximum reaching roughly 30 at%, whereas the Se concentration drops by greater than 20%. Outside these, the former rapidly decreases and a compositional ratio of Sn to Se atom remains nearly constant at unity. The typical thickness of surface SnOx layer at GBs is about 15 nm in the untreated SnSe sample according to both STEM and APT observations. Even nanoscale GB phases could considerably affect charge21 and thermal22 transport properties of materials, consequently inhibiting the observation of intrinsic values21,22.
A typical HAADF–STEM image for the purified SnSe sample does not show the presence of SnOx at the GBs (Fig. 3i). The magnified image focusing on the GB shows that two adjacent crystalline grains form the tightly jointed interface without intervening secondary phases (Fig. 3j). The three-dimensional APT reconstruction (Fig. 3k) and one-dimensional compositional profile extracted across the GB (Fig. 3l) show that the distribution of Sn and Se atoms is nearly homogeneous at the same level over the specimen with a negligible discontinuity across the GB. No signal for the presence of O atoms is detected in the mass-to-charge ratio spectrum (Fig. 3m). The results confirm that our purification process effectively removes surface SnOx from SnSe-based materials.
The strong beneficial effect of our purification process is dramatically evident in the thermoelectric properties of polycrystalline SnSe. Because of the characteristic lamellar structure of SnSe (Fig. 4a), its thermoelectric properties are highly anisotropic9. Namely, polycrystalline and single-crystal samples exhibit the lowest thermal conductivity (κ) along the parallel direction of compaction (//) and along the crystallographic a axis9, respectively. Along these directions, we compare κ of our polycrystalline SnSe-based samples with the reported values for the undoped single-crystal sample9. To obtain accurate κ, we directly recorded the temperature-dependent heat capacity (Cp) of the samples over the entire temperature range using differential scanning calorimetry (DSC). To ensure the credibility of data, we ran measurements for more than 20 samples. The Cp values taken at the three different heating rates of 5, 7.5 and 10 K min−1, respectively, unambiguously confirm that they are nearly constant outside the phase transition temperature of the Na0.03Sn0.965Se sample regardless of the heating rate (Fig. 4b). We averaged the obtained Cp values and then derived the κ. The averaged experimental Cp is comparable to the modelled value derived from the previous report10 over the entire range of temperature.
Ultralow thermal conductivity
The purification process reduces lattice thermal conductivity (κlat) for the polycrystalline SnSe sample and makes it comparable to that reported for single crystals over the entire temperature range (Fig. 4c). In contrast, when SnSe powder is treated only by the post H2-reduction without the Sn metal purification, the decrease in κlat is small. The κlat values for the untreated, H2-reduced and purified polycrystalline SnSe samples are roughly 1.03, 0.99 and 0.58 W m–1 K–1 at 300 K and roughly 0.39, 0.38 and 0.23 W m–1 K–1 at 773 K, respectively. This observation confirms that the application of a proper Sn purification procedure is essential to unveil the intrinsically ultralow κlat in SnSe-based thermoelectric materials.
Hole-doped NaxSn0.995−xSe (x = 0.01–0.03) purified samples exhibit even lower κlat than the undoped polycrystalline and single-crystal SnSe samples. Their κlat decreases with the higher Na concentration because of slightly softened phonon frequency (Fig. 4d and Supplementary Fig. 6). The lowest κlat is roughly 0.17 (x = 0.01), 0.12 (x = 0.02) and 0.07 W m–1 K–1 (x = 0.03) at 783 K, in comparison with roughly 0.20 W m–1 K–1 at 973 K for the single-crystal SnSe along the a axis9. The observed value is one of the lowest κlat reported for bulk crystalline solids. In comparison, bulk polycrystalline CsAg5Te3 exhibits roughly 0.18 W m–1 K–1 at 727 K (ref. 23) and disordered thin films of lamellar WSe2, prepared by the vacuum deposition, give roughly 0.05 W m–1 K–1 at 300 K (ref. 24). The x = 0.03 sample shows the lowest total thermal conductivity (κtot) among the series as the trend of κlat (Supplementary Fig. 7). Its κtot at 300 K is higher at roughly 0.65 than 0.46 W m–1 K–1 of the single-crystal SnSe sample. They show comparable κtot at the elevated temperatures, and the former exhibits a lower minimum of roughly 0.21 W m–1 K–1 at 783 K than roughly 0.23 W m–1 K–1 at 773 K of the latter.
The ultralow κ of NaxSn0.995−xSe and SnSe samples up to 783 K is present before the sharp endothermic thermal event occurs, thus the phase transition has a negligible effect on the ultralow value of κ. Figure 4e demonstrates that the temperature-dependent κtot calculated by our DSC Cp and modelled Cp derived from the previous report10 are comparable from 300 to 783 K, confirming that κ is not underestimated by the modelled Cp in this temperature regime.
We prepared ten independent Na0.03Sn0.965Se specimens and cross-checked the reproducibility of the ultralow κ from two institutions, SNU and Northwestern University, and the manufacturer of Netzsch Instruments (Fig. 4f). The measurements on all specimens (four from SNU, three from Northwestern University and three from Netzsch) gave the uncertainty in κtot of less than roughly 10% in the temperature range 323–773 K.
Charge transport properties
The effect of the purification process is seemingly marginal on electrical conductivity (σ) for the undoped polycrystalline SnSe samples (Supplementary Fig. 8a) because such samples have a very low carrier concentration (nH), for example, roughly 2.5 × 1017 and 2.0 × 1017 cm−3 at 300 K for the untreated and purified polycrystalline SnSe, respectively. In the doped NaxSn0.995−xSe samples with nH roughly 1019 cm−3, however, the purification process that minimizes surface SnOx is key to achieving the enhanced Hall carrier mobility (μH) (Supplementary Fig. 9) and σ over the full range of temperature (Fig. 5a). The σ markedly increases with the higher Na content in the temperature range 300–523 K. This leads to the enhanced thermoelectric performance of the samples in the low- to mid-temperature regime, a big improvement over previous polycrystalline SnSe thermoelectrics that suffer from low σ in that range, resulting in poor ZT values. The x = 0.03 sample shows the σ of 140 and 118 S cm–1 at 423 and 783 K measured parallel to the SPS direction, and 181 and 132 S cm–1 at the same temperatures perpendicular to the SPS direction.
The Seebeck coefficients (S) of the NaxSn0.995−xSe samples are nearly the same along the parallel and perpendicular direction of SPS (Supplementary Fig. 10). Because of the higher hole concentration, the S values are lower than in the undoped SnSe samples (Fig. 5b). S slightly increases with the higher Na concentration consistent with the multi-band nature of the valence band in this material, which enhances the effective hole mass with higher hole concentrations as the Fermi level lowers to cross several valence bands according to our theoretical calculations (Supplementary Fig. 11) and the previous report10. Their S is slightly increased by our purification process making the Na doping more effective. For example, the maximum S for the x = 0.03 sample is +322 and +342 μV K–1 at 673 K before and after the purification process, respectively. The high reproducibility of σ and S values were confirmed using numerous independently synthesized specimens (Supplementary Fig. 12).
The simultaneously increased σ and S of the purified NaxSn0.995−xSe samples result in the improved power factor (Fig. 5c) that trends higher with the rising Na concentration. The x = 0.03 sample exhibits power factors near 9 μW cm–1 K–2 in the wide range of temperature 473–783 K with a maximum of roughly 9.62 μW cm–1 K–2 at 498 K parallel to the SPS direction. The maximum power factor is roughly 12.06 μW cm–1 K–2 at 473 K perpendicular to the SPS direction, which is the highest value reported for polycrystalline SnSe-based materials.
Thermoelectric figure of merit
The purification process concurrently enhances σ and S, and decreases κtot for the NaxSn0.995−xSe samples, leading to an extraordinarily high thermoelectric figure of merit ZT. It increases with higher Na concentration. The x = 0.03 sample exhibits the maximum ZT (ZTmax) roughly 3.1 at 783 K, which is the highest reported for any thermoelectric system. This ultrahigh thermoelectric performance is attained below the phase transition temperature as observed in our DSC results (Fig. 4b), affirming no overestimation of ZT by the phase transition. In comparison, p- and n-type SnSe single crystals exhibit a ZTmax of roughly 2.6 at 923 K (ref. 9) and 2.8 at 773 K (ref. 11), respectively (Fig. 5d). Among the highest performance polycrystalline thermoelectric systems have been PbTe-8%SrTe doped with 2% Na (ZTmax roughly 2.5 at 923 K, ref. 8) and ball-milled and H2-reduced SnSe-5%PbSe doped with 1% Na (ZTmax roughly 2.5 at 773 K, ref. 12). ZT for Na0.03Sn0.965Se already exceeds unity above 473 K, at which temperature regime few materials show comparable performance. It exhibits a record-high average ZT25 roughly 2.0 from 400 to 783 K (Supplementary Fig. 13). The deviation in temperature-dependent ZT values on consecutive heating and cooling cycles is less than 10%, indicating the prospect of stable operation from 300 to 783 K for thermoelectric power generation (Supplementary Figs. 14 and 15).
We conclude that a trace of SnOx in the starting tin metal reagent, used to prepare SnSe samples, has persistently concealed the intrinsic charge and thermal transport properties of SnSe and prevented the full thermoelectric performance from being realized. When properly purified and doped using the methods described above, polycrystalline SnSe exhibits an extraordinarily high ZT of roughly 3.1, outperforming any other bulk thermoelectric systems. The ultrahigh thermoelectric performance indeed originates from the intrinsic crystal chemistry of this simple yet remarkable binary compound SnSe, and this bodes well for the future development of this material to affect power generation applications from waste heat. This revelation has broader implications of how other systems need to be handled in the future and calls for the re-examination of synthesis and sample preparation processes for extensively studied thermoelectric systems, especially those containing tin.
Methods
Note
All procedures for the synthesis and sample preparations were strictly carried out in an Ar-filled glovebox (99.99% purity), in which the levels of moisture and oxygen are kept at 0 and less than 1 ppm, respectively, unless noted otherwise. When samples were transported from the glovebox for measurements and compaction processes, they were properly protected under a mobile Ar flowing system.
Reagents
The following starting reagents were used as received unless noted otherwise: Se shot (99.999%, 5N Plus) and Na piece (99.9%, Sigma-Aldrich). As-received Sn chunk (99.999%, American Elements) was used to synthesize ‘untreated’ SnSe-based materials as control samples. It was purified by our melting-purification process as described below to eliminate surface tin oxides, and was used to synthesize ‘purified’ SnSe-based materials.
Purification of Sn
As-received Sn chunks were apparently silvery. They were placed on a graphite sheet prewashed with ethanol, and were heated at 473 K, which is near the melting point of Sn at roughly 505 K, for 6 h under a 4% H2/96% Ar with a flow rate of 200 ml min–1. A change in their surface colour and lustre was invisible. The resulting Sn chunks were loaded into a carbon-coated and evacuated fused-silica tube (roughly 10–4 Torr). The tube was heated at 1,273 K for 6 h, followed by cooling to room temperature. Ash-like black residues formed at the top and surface of the Sn ingot. They were identified as tin oxides by Fourier transformed far-infrared absorption spectroscopy. They were scraped out of the Sn ingot. The same melting-purification process was repeated three times at 873–723 K until the black residues were no longer observed.
Synthesis
Purified and untreated materials with the nominal compositions NaxSn0.995–xSe (x = 0.01–0.03) and SnSe as a reference were synthesized by reacting stoichiometric mixtures of proper starting reagents. They were loaded in carbon-coated and evacuated fused-silica tubes (roughly 10–4 Torr), and were heated at 1,223 K for 12 h, followed by quenching to ice water. The obtained ingots were further annealed at 773 K for 48 h and were cooled naturally to room temperature. The weight of typical ingots was approximately 13 g. They were pulverized by hand-grinding, and were subsequently purified at 613 K for 6 h under a 4% H2/96% Ar with a flow rate of 200 ml min−1.
Compacting powders
The resulting powders were loaded in a BN-coated graphite die and were cold-pressed manually in an Ar-filled glovebox. To avoid any possible oxidation of a sample, the loaded die was tightly sealed in a plastic zipper bag and taken out of the glovebox. It was transported from the chamber of the glovebox to the adjacently placed SPS system (SPS-211Lx, Fuji Electronic Industrial Co.) under a mobile Ar (99.99%) flowing system. Powder samples in the die were densified at roughly 783 K for 5 min under an axial pressure of 50 MPa in a vacuum of roughly 1.4 × 10−2 Torr using SPS. All SPS-processed samples show relative densities of roughly 96%.
Powder X-ray diffraction
We carried out X-ray diffraction analysis on a SmartLab Rigaku X-ray diffractometer with Cu Kα (λ = 1.5418 Å) graphite-monochromatized radiation operating at 40 kV and 30 mA at room temperature. The patterns measured parallel and perpendicular to the pressing direction of the SPS-processed ingots for purified and untreated SnSe and Na0.03Sn0.965Se samples are given in Supplementary Figs. 16 and 17.
TOF–SIMS
TOF–SIMS experiments were carried out on a Physical Electronics TRIFT III spectrometer. The SPS-processed samples were polished with Buehler Ecomet III Tabletop Polisher/Grinder to prepare a smooth surface. Subsequently, they were sputtered with a 5 keV Ar ion beam for 5 min in SIMS chamber to expose the GB. During this process, omnipresent H2O even in an ultrahigh vacuum chamber was ionized to give H+, which then attached to surface tin oxides to form SnOH+. Accordingly, to examine the distribution of surface tin oxides, the SnOH+ ion mapping images were collected for 10 min. The primary ion source of SIMS is gallium beam with 25 keV energy. The measurements were conducted in NUANCE-Keck-II centre of Northwestern University.
Hall measurements
The Hall coefficients (RH) were obtained by the Van der Pauw method on a Lake Shore HMS8407 Hall effect measurement system in a magnetic field of 1.5 T and 3 mA excitation current. The hole carrier concentration (nH) and hole mobility (μH) were accessed by the formulas, nH = 1/(eRH) and μH = RHσ, respectively.
Electrical and thermal transport property measurements
The obtained SPS-processed pellets were cut and polished into a rectangular shape with a length of 13 mm and thickness of roughly 2 mm under a N2 atmosphere (99.99% purity) (Supplementary Fig. 18). The electrical conductivity and Seebeck coefficient were measured simultaneously under an Ar atmosphere from room temperature to 823 K using a Netzsch SBA 458 Nemesis system. A Netzsch LFA 457 MicroFlash instrument was used to record the thermal diffusivity of the samples coated with graphite. The typical samples are disc shaped with a diameter of 8 mm and thickness ranging from 1 to 2 mm. To confirm the reproducibility of ultralow thermal conductivity of the Na0.03Sn0.965Se samples, the thermal diffusivity was cross-checked at Northwestern University and Netzsch Instruments (Korea) using LFA 457 and 467 instruments, respectively (Supplementary Figs. 19–21). The thermal conductivity was calculated from the formula κtot = DCpρ, where D is the thermal diffusivity, Cp is the heat capacity, which was directly measured using the DSC technique, and ρ is the mass density of the specimens. The ρ value used was obtained by their geometrical dimensions and masses, which is nearly the same as that by the Archimedes method. The density values used are given in Supplementary Table 1. The total thermal conductivity κtot is the sum of the lattice (κlat) and electronic thermal (κele) conductivities. κele is proportional to the electrical conductivity (σ) according to the Wiedemann–Franz relation (κele = LσT), where L is the temperature-dependent Lorenz number and T is the absolute temperature. The κlat value was calculated by subtracting the κele from the κtot value by the relation κlat = κtot – κele. Average ZT (ZTave) was calculated using the following equation25:
where Thot and Tcold represent the temperature at the hot and cold sides, respectively.
Heat capacity measurements
The temperature-dependent heat capacity (Cp) was experimentally recorded by differential scanning calorimeter (DSC Polyma 214, Netzsch). To minimize the error, samples were cut into a cube with dimensions of roughly 2 × 2 × 2 mm3. Because Na easily reacts with typical Al2O3 or Al crucibles, Pt crucibles were used. Before the measurement, the blank crucible was heated to 823 K at least twice under a high-purity argon (99.999%) flow to remove any possible residual water and physisorbed O2. Afterwards, a standard sapphire disc with a diameter of 4 mm and a thickness of 0.25 mm was loaded into the crucible and measured up to 823 K. Subsequently, the standard sapphire was taken out, and the Na0.03Sn0.965Se sample was placed in the same crucible. The loaded crucible was purged with a high-purity argon flow for 30 min to ensure a dry and air-free atmosphere before the measurement. The Cp was extracted by comparing the signal difference between the reference sapphire and sample26.
STEM
STEM specimens were excised from the GB using a dual-beam scanning electron microscope/focused ion beam (Helio NanoLab 650, FEI) system using gallium ion milling. Before the ion milling, the surface of specimens was protected with carbon coating by sputtering. Structures and chemical compositions around GBs were analysed using a spherical aberration-corrected JEM ARM-200F microscope (Cold FEG Type, JEOL) equipped with an SDD type energy-dispersive X-ray spectroscopy (EDS) detector (Solid Angle 0.9-sr, X-MaxN 100TLE, Oxford) at 200 kV installed at the National Centre for Inter-University Research Facilities in SNU. In HAADF–STEM images, the point-to-point resolution was approximately 80 pm after correcting the spherical aberration, and the angular range of the annular detector used was from 68 to 280 mrad. All STEM images were recorded using a high-resolution CCD detector with a 2,000 × 2,000-pixel device in the GIF-QuantumER imaging filter (Gatan). For STEM–EDS investigation, chemical maps were acquired with a probe size of 0.13 nm and a probe current of 40 pA.
APT
APT needle-shaped specimens were prepared using a dual-beam scanning electron microscope/focused ion beam (Helios NanoLab 650, FEI) following the site-specific ‘lift-out’ method27. The specimens were measured in a local electrode atom probe (LEAP 4000 X Si, Cameca) with voltage- and laser-assisted evaporation modes for the Sn reagent and SnSe samples, respectively. For a voltage mode, a voltage pulse with a repetition rate of 200 kHz and pulse fraction of 20% was used. The detection rate was five ions per 1,000 pulses (0.5%) on average. The base temperature of specimen was 30 K. For a laser mode, a 5 pJ ultraviolet (wavelength, 355 nm) laser with 10 ps pulse and a 200 kHz repetition rate was used. The detection rate was one ion per 100 pulses (1%) on average. For both modes, the base temperature was 40 K and the ion flight path was 160 mm. The detection efficiency was limited to 50% due to the open area of the microchannel plate. The APT data were processed using the software package IVAS v.3.8.0 (ref. 18).
Calculations for phonon band structure and Grüneisen parameters
Phonon band structure and Grüneisen parameters were calculated within quasi-harmonic approximations based on DFT calculations. They have been calculated for pristine SnSe previously9. In this work, we further calculated them for the optimally hole-doped system, namely, Na0.03Sn0.97Se. To obtain accurate force constant matrix, we used a 2 × 2 × 2 supercell for Na0.03Sn0.97Se with 64 atoms, and accordingly the supercell accommodates 512 atoms in total. For better comparison, we also considered the same size of supercell for pristine SnSe. DFT force calculations were performed with a plane wave set of 350 eV energy cutoff, gamma point k-space sampling and PBEsol exchange functional28, and they were forced to converge until the largest component of atomic force becomes smaller than 10–8 eV Å–1. To evaluate the Grüneisen parameters defined by the relation , where V is the volume of unit cell and ωi is frequency of i-th phonon mode, we considered three sets of phonon dispersion relation with different volumes, namely, 0.99, 1.00 and 1.01 times the optimized volume of the unit cell. Calculation results are presented in Supplementary Fig. 6.
Calculations for electronic band structure
To understand the enhanced Seebeck coefficient by Na doping, we obtained electronic band structures for hole-doped Na0.03Sn0.97Se and pristine SnSe using DFT calculations with plane wave basis set with 350 eV energy cutoff, 4 × 4 × 4 k-space sampling, and SCAN + rVV10 functional29. We used a × 1 supercell, and the lattice parameters and internal coordinates were fully optimized. On Na doping, the lattice dimension decreases by about 0.5% along the b and c axes and increases by about 0.3% along the a axis.
It should be noted that the recent investigation by angle-resolved photon emission spectroscopy (ARPES) for SnSe clearly shows the emergence of pudding mould-type bands near valence band maximum30, which is highly important for achieving high power factor within the band convergence strategy. However, many previous DFT studies for SnSe using semilocal exchange-correlation functional such as Perdew–Burke–Ernzerhof (PBE) generalized gradient approximation could not reproduce band structures observed by the ARPES appropriately. In this work, we found that such band dispersions in SnSe seen by the ARPES experiments can be well reproduced by SCAN + rVV10 functional. Accordingly, we applied the same method to hole-doped Na0.03Sn0.97Se. We considered a 64-atom-containing supercell for both SnSe and Na0.03Sn0.97Se. Band structures are evaluated along a high-symmetric line in k-space. For density of states, we used a denser 10 × 10 × 10 regular mesh. Calculation results are given in Supplementary Fig. 11.
Online content
Any methods, additional references, Nature Research reporting summaries, source data, extended data, supplementary information, acknowledgements, peer review information; details of author contributions and competing interests; and statements of data and code availability are available at 10.1038/s41563-021-01064-6.
Supplementary information
Acknowledgements
The work at SNU was supported by the National Research Foundation of Korea (NRF) grant funded by the Korean Government (MSIT) (no. NRF-2020R1A2C2011111), Nano Material Technology Development Program through the NRF grant funded by the Korean Government (MSIP) (nos. NRF-2017M3A7B4049274 and NRF-2017M3A7B4049273), the IBS (grant no. IBS-R009-G2) and LG Chem. The Northwestern personnel and research work were supported by the Department of Energy, Office of Science, Basic Energy Sciences under grant no. DE-SC0014520. The work at Northwestern was supported by the Department of Energy, Office of Science, Basic Energy Sciences under grant no. DE-SC0014520 (materials characterization and physical properties measurements). This work also made use of the EPIC and Keck facilities of Northwestern University’s NUANCE Centre, which has received support from the Soft and Hybrid Nanotechnology Experimental Resource (grant no. NSF ECCS-1542205); the MRSEC program (grant no. NSF DMR-1720139) at the Materials Research Centre; the International Institute for Nanotechnology (IIN); the Keck Foundation and the State of Illinois, through the IIN. Parts of the text in this work have been reproduced from the thesis by Y.K.L., at SNU, and is accessible at https://s-space.snu.ac.kr/bitstream/10371/169453/1/000000162714.pdf.
Source data
Author contributions
M.G.K. and I.C. conceived and designed the experiments. C.Z., Y.K.L., S.B., H.L., B.G. and I.C. synthesized the samples and characterized their properties. Z.-Z.L. and M.G.K. cross-checked thermoelectric properties. X.C. and V.P.D. performed TOF–SIMS characterizations, and contributed to overall interpretation of data and their implications. Y.Y., J.Y.L., O.C.M. and M.W. collected APT data. Y.-L.L., H.C. and J.I. carried out theoretical calculations. S.-P.C. performed TEM characterizations. M.G.K. and I.C. wrote the manuscript with discussion and input from all authors.
Data availability
The datasets for Figs. 1–5 are available in the source data section. Additional information is available from the authors on request. Source data are provided with this paper.
Code availability
The computer codes that support the findings of this study are available from the corresponding author on reasonable request.
Competing interests
The authors declare no competing interests.
Footnotes
Peer review informationNature Materials thanks Baptiste Gault and the other, anonymous, reviewer(s) for their contribution to the peer review of this work.
Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.
These authors contributed equally: Chongjian Zhou, Yong Kyu Lee, Yuan Yu.
Contributor Information
Mercouri G. Kanatzidis, Email: m-kanatzidis@northwestern.edu
In Chung, Email: inchung@snu.ac.kr.
Supplementary information
The online version contains supplementary material available at 10.1038/s41563-021-01064-6.
References
- 1.Gingerich DB, Mauter MS. Quantity, quality, and availability of waste heat from United States thermal power generation. Environ. Sci. Technol. 2015;49:8297–8306. doi: 10.1021/es5060989. [DOI] [PubMed] [Google Scholar]
- 2.Jood P, Ohta M, Yamamoto A, Kanatzidis MG. Excessively doped PbTe with Ge-induced nanostructures enables high-efficiency thermoelectric modules. Joule. 2018;2:1339–1355. doi: 10.1016/j.joule.2018.04.025. [DOI] [Google Scholar]
- 3.Tan G, Zhao L-D, Kanatzidis MG. Rationally designing high-performance bulk thermoelectric materials. Chem. Rev. 2016;116:12123–12149. doi: 10.1021/acs.chemrev.6b00255. [DOI] [PubMed] [Google Scholar]
- 4.He, J. & Tritt, T. M. Advances in thermoelectric materials research: looking back and moving forward. Science357, eaak9997 (2017). [DOI] [PubMed]
- 5.Biswas K, et al. High-performance bulk thermoelectrics with all-scale hierarchical architectures. Nature. 2012;489:414–418. doi: 10.1038/nature11439. [DOI] [PubMed] [Google Scholar]
- 6.Tang Y, et al. Convergence of multi-valley bands as the electronic origin of high thermoelectric performance in CoSb3 skutterudites. Nat. Mater. 2015;14:1223–1228. doi: 10.1038/nmat4430. [DOI] [PubMed] [Google Scholar]
- 7.Hinterleitner B, et al. Thermoelectric performance of a metastable thin-film Heusler alloy. Nature. 2019;576:85–90. doi: 10.1038/s41586-019-1751-9. [DOI] [PubMed] [Google Scholar]
- 8.Tan G, et al. Non-equilibrium processing leads to record high thermoelectric figure of merit in PbTe–SrTe. Nat. Commun. 2016;7:12167. doi: 10.1038/ncomms12167. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 9.Zhao L-D, et al. Ultralow thermal conductivity and high thermoelectric figure of merit in SnSe crystals. Nature. 2014;508:373–377. doi: 10.1038/nature13184. [DOI] [PubMed] [Google Scholar]
- 10.Zhao L-D, et al. Ultrahigh power factor and thermoelectric performance in hole-doped single-crystal SnSe. Science. 2016;351:141–144. doi: 10.1126/science.aad3749. [DOI] [PubMed] [Google Scholar]
- 11.Chang C, et al. 3D charge and 2D phonon transports leading to high out-of-plane ZT in n-type SnSe crystals. Science. 2018;360:778–783. doi: 10.1126/science.aaq1479. [DOI] [PubMed] [Google Scholar]
- 12.Lee YK, Luo Z, Cho SP, Kanatzidis MG, Chung I. Surface oxide removal for polycrystalline SnSe reveals near-single-crystal thermoelectric performance. Joule. 2019;3:719–731. doi: 10.1016/j.joule.2019.01.001. [DOI] [Google Scholar]
- 13.Wei W, et al. Achieving high thermoelectric figure of merit in polycrystalline SnSe via introducing Sn vacancies. J. Am. Chem. Soc. 2018;140:499–505. doi: 10.1021/jacs.7b11875. [DOI] [PubMed] [Google Scholar]
- 14.Lee YK, et al. Enhancing p-type thermoelectric performances of polycrystalline SnSe via tuning phase transition temperature. J. Am. Chem. Soc. 2017;139:10887–10896. doi: 10.1021/jacs.7b05881. [DOI] [PubMed] [Google Scholar]
- 15.Wei PC, et al. The intrinsic thermal conductivity of SnSe. Nature. 2016;539:E1–E2. doi: 10.1038/nature19832. [DOI] [PubMed] [Google Scholar]
- 16.Zhao L-D, Chang C, Tan G, Kanatzidis MG. SnSe: a remarkable new thermoelectric material. Energy Environ. Sci. 2016;9:3044–3060. doi: 10.1039/C6EE01755J. [DOI] [Google Scholar]
- 17.Roy S, Joshi AG, Chatterjee S, Ghosh AK. Local symmetry breaking in SnO2 nanocrystals with cobalt doping and its effect on optical properties. Nanoscale. 2018;10:10664–10682. doi: 10.1039/C7NR07427A. [DOI] [PubMed] [Google Scholar]
- 18.Yu Y, et al. Revealing nano-chemistry at lattice defects in thermoelectric materials using atom probe tomography. Mater. Today. 2020;32:260–274. doi: 10.1016/j.mattod.2019.11.010. [DOI] [Google Scholar]
- 19.Ye X, et al. Magnetoelectric tuning of pinning-type permanent magnets through atomic-scale engineering of grain boundaries. Adv. Mater. 2021;33:2006853. doi: 10.1002/adma.202006853. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 20.Gault, B., Moody, M. P., Cairney, J. M. & Ringer, S. P. Atom Probe Microscopy (Springer Science & Business Media, 2012).
- 21.Slade TJ, et al. Understanding the thermally activated charge transport in NaPbmSbQm+2 (Q = S, Se, Te) thermoelectrics: weak dielectric screening leads to grain boundary dominated charge carrier scattering. Energy Environ. Sci. 2020;13:1509–1518. doi: 10.1039/D0EE00491J. [DOI] [Google Scholar]
- 22.Kuo JJ, Wood M, Slade TJ, Kanatzidis MG, Snyder GJ. Systematic over-estimation of lattice thermal conductivity in materials with electrically-resistive grain boundaries. Energy Environ. Sci. 2020;13:1250–1258. doi: 10.1039/C9EE03921J. [DOI] [Google Scholar]
- 23.Lin H, et al. Concerted rattling in CsAg5Te3 leading to ultralow thermal conductivity and high thermoelectric performance. Angew. Chem. Int. Ed. 2016;55:11431–11436. doi: 10.1002/anie.201605015. [DOI] [PubMed] [Google Scholar]
- 24.Chiritescu C, et al. Ultralow thermal conductivity in disordered, layered WSe2 crystals. Science. 2007;315:351–353. doi: 10.1126/science.1136494. [DOI] [PubMed] [Google Scholar]
- 25.Qin B, et al. Ultrahigh average ZT realized in p-type SnSe crystalline thermoelectrics through producing extrinsic vacancies. J. Am. Chem. Soc. 2020;142:5901–5909. doi: 10.1021/jacs.0c01726. [DOI] [PubMed] [Google Scholar]
- 26.Rudtsch S. Uncertainty of heat capacity measurements with differential scanning calorimeters. Thermochim. Acta. 2002;382:17–25. doi: 10.1016/S0040-6031(01)00730-4. [DOI] [Google Scholar]
- 27.Miller MK, Russell KF. Atom probe specimen preparation with a dual beam SEM/FIB miller. Ultramicroscopy. 2007;107:761–766. doi: 10.1016/j.ultramic.2007.02.023. [DOI] [PubMed] [Google Scholar]
- 28.Perdew JP, et al. Restoring the density-gradient expansion for exchange in solids and surfaces. Phys. Rev. Lett. 2008;100:136406. doi: 10.1103/PhysRevLett.100.136406. [DOI] [PubMed] [Google Scholar]
- 29.Peng H, Yang ZH, Perdew JP, Sun J. Versatile van der Waals density functional based on a meta-generalized gradient approximation. Phys. Rev. X. 2016;6:041005. [Google Scholar]
- 30.Pletikosić I, et al. Band structure of the IV-VI black phosphorus analog and thermoelectric SnSe. Phys. Rev. Lett. 2018;120:156403. doi: 10.1103/PhysRevLett.120.156403. [DOI] [PubMed] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Supplementary Materials
Data Availability Statement
The datasets for Figs. 1–5 are available in the source data section. Additional information is available from the authors on request. Source data are provided with this paper.
The computer codes that support the findings of this study are available from the corresponding author on reasonable request.